top of page

ISO 5173
Bend Tests on Welds in Metallic Materials

ISO 5173 roller bend fixture with interchangeable formers for weld bend tests by Universal Grip

Downloads: ISO 5173 Roller Bend Fixture for Weld Bend Tests – Universal Grip Data Sheet (PDF)

Written by Chris Thomas, Universal Grip Company · Reviewed by Frank Bertini · Updated October 31, 2026

ISO 5173 is the international test method for bend tests on welded joints in metallic materials. It tells you how to cut, machine and bend transverse root, face and side bend specimens, longitudinal bend specimens and cladding specimens so that imperfections on or near the stretched surface open up where an inspector can see them. Welding engineers, welder-qualification bodies, pressure-equipment fabricators and third-party labs use it every day, usually because an application standard such as ISO 15614-1 or ISO 9606-1 calls for it. It looks simple, but it is easy to get wrong: the former diameter depends on parent metal elongation, roller spacing has a tolerance window, edges must be rounded within limits, and thick face and root bends need far more force than most people expect. This guide covers the current edition, specimen types and dimensions, the formulas for former diameter and roller spacing, how to size the test machine, a step-by-step procedure, worked calculations, common errors and the equivalent ASTM methods, plus the bend testing fixtures and machines that do the job.

ISO 5173 at a glance

  • Current edition: ISO 5173:2023 (fourth edition), which replaces ISO 5173:2009 and its Amendment 1:2011. Adopted in Europe as EN ISO 5173:2023.

  • Scope: transverse root, face and side bend tests on butt welds, butt welds with cladding (welds in clad plates and clad welds) and cladding without butt welds, plus guided roller and longitudinal bend tests as alternatives for joints whose parent metal, HAZ and weld metal bend very differently. Applies to metallic materials in all product forms and any welding process.

  • Purpose: to reveal imperfections on or near the tension surface and/or to assess ductility.

  • Specimen: machined strip with the weld at mid-length; thickness usually full plate thickness up to 30 mm, or 10 ± 0.5 mm for side bends and reduced specimens.

  • Loading: three-point bending with a former between two rollers, a U-type plunger and die, a wrap-around roller method, or with a backing plate.

  • Bend angle: set by the application standard; otherwise about 180°.

  • Speed: not specified numerically; keep it constant and record it if known.

  • Result: visual examination of the outer surface and sides after bending, judged against the acceptance criteria of the application standard; optionally bending elongation.

  • Related standards: ISO 7438 (bend test on metallic materials), ISO 15614-1 and ISO 9606-1 (application standards), ASTM E190 and ASTM E290 (US methods).

What the ISO 5173 bend test measures and who uses it

A bend test is a pass or fail ductility and soundness check. Bending stretches one surface well past yield, so lack of fusion, porosity, slag, cracks and brittle zones open up as visible defects. ISO 5173 sets no acceptance criteria; the application standard decides how big an opening is allowed and how many specimens you need.

  • Welding procedure qualification: ISO 15614-1 (steels and nickel alloys) and ISO 15614-2 (aluminium) call up ISO 5173 bend tests alongside transverse tensile, impact, macro and hardness tests.

  • Welder qualification: ISO 9606-1 and related parts use bend tests as one of the ways to examine a welder's test piece.

  • Production and pressure-equipment QC: bend tests on production coupons confirm a procedure still delivers sound, ductile welds.

  • Cladding and overlay: face and side bends check bonding and deposit soundness.

Specimen types in ISO 5173:2023

  • TFBB: transverse face bend on a butt weld, weld face in tension.

  • TRBB: transverse root bend on a butt weld, root in tension.

  • TSBB: transverse side bend on a butt weld, the weld cross-section in tension.

  • LFBB and LRBB: longitudinal face and root bends on a butt weld, with the weld running along the specimen.

  • FBC and SBC: face and side bends on cladding without a butt weld.

  • FBCB and SBCB: face and side bends on cladding with a butt weld.

Specimen dimensions and preparation

Thickness

  • Transverse face and root bends (TFBB, TRBB): specimen thickness ts equals the parent metal thickness, up to 30 mm. If the plate is thicker than 10 mm, the specimen may be machined from one side only to 10 ± 0.5 mm, keeping the surface that will be in tension. Several specimens may be needed to cover the full thickness.

  • Transverse side bends (TSBB): ts = 10 ± 0.5 mm. If the joint is thicker than 40 mm, the full-thickness width may be split into several specimens.

  • Longitudinal bends (LFBB, LRBB): ts equals the adjacent parent thickness but should not exceed 10 mm; machining to 10 ± 0.5 mm is allowed when the plate is thicker.

  • Cladding specimens: FBC and FBCB use ts = tw + tc (parent under the cladding plus cladding thickness), not exceeding 10 mm; SBC and SBCB use ts = 10 ± 0.5 mm.

Width

  • Plates, transverse face and root bends: b ≥ 4 ts unless the application standard says otherwise.

  • Pipes: for outside diameter D from 25 mm to 50 mm, b = t + 0.1 D (minimum 8 mm); above 50 mm, b = t + 0.05 D (minimum 8 mm, and it should not exceed 40 mm). Below 25 mm, specimens may be cut from half or quarter sections of the pipe. When D is more than 25 times the wall thickness, use the plate rules.

  • Side bends: width equals the adjacent parent thickness.

  • Longitudinal bends: b = Ls + 2 b1, where Ls is the maximum weld width after machining and b1 = 15 mm.

Length, edges and surface

  • Total length: Lt ≥ l + 2R, where l is the roller spacing and R the roller radius.

  • Edge radius: tension-face edges may be rounded to r ≤ 0.2 ts, with a maximum of 3 mm, without burrs or transverse marks. Unrounded edges are accepted if the result is satisfactory.

  • Surface: machine or grind so the metal is not work-hardened or overheated. Within the span l there must be no transverse scratches or notches, except undercut that the application standard requires you to keep. Excess weld metal (cap and root reinforcement) is removed flush unless otherwise specified.

  • Extraction: material affected by thermal cutting or shearing must be machined away. Mark every specimen so its position in the test piece can be traced.

  • Heat treatment: none unless the application standard requires or permits it. Record any treatment, including hydrogen-removal treatments, and for naturally ageing aluminium alloys record the time between welding and testing.

Conditioning and test temperature

ISO 5173 has no conditioning period like a plastics or rubber standard. Tests are normally run at room temperature, and the test temperature is recorded. Follow the application standard if it asks for something different. The only time-based control is for naturally ageing aluminium alloys, where the delay between welding and bending must be recorded.

Former diameter, roller spacing and machine requirements

Former diameter d

  • Steel, nickel and nickel alloys: d = 4 ts when the minimum specified elongation A of the parent metal is 20 % or more.

  • When A is less than 20 %: d = (100 × ts / A) − ts, unless the application standard specifies something else.

  • Aluminium alloys: the same formula applies when A is above 5 %. When A is 5 % or less, the specimen is annealed to its lowest-strength condition and d is calculated from the annealed elongation.

  • Dissimilar joints: use the lowest A of the materials involved.

  • Which A: use the minimum elongation required by the parent metal specification, not the value printed on the mill certificate.

Rollers and spacing

  • Roller radius: R ≥ 20 mm.

  • Roller spacing for the former method: d + 2 ts + 1 ≤ l ≤ d + 3.5 ts (mm).

  • With a backing plate of thickness tb: d + 2(ts + tb) + 1 ≤ l ≤ d + 3.5(ts + tb).

  • U-type jig: plunger radius rP = d/2 and die radius rD = rP + ts + 2 (dimensions in mm).

  • Wrap-around roller method: the initial distance from roller contact to the weld centre line Lf lies between 0.7 d and 0.9 d.

Speed and machine

ISO 5173 gives no numerical test speed. The load is applied slowly and continuously, perpendicular to the specimen surface, with the weld centred under the former, and the speed should be kept constant and recorded when known. Any rigid universal testing machine or press with enough capacity and stroke will do, but a machine with a controlled crosshead speed, a force readout and position data gives you a repeatable bend and lets you calculate the bend angle from former displacement as described in ISO 7438.

The Universal Grip ISO 5173 bend fixture

Our ISO 5173 bend fixture (part ref. UGC-ISO5173-BF) is a roller bend fixture for transverse and longitudinal bend testing of welded joints. The specimen rests on two support rollers whose spacing is set on a graduated base, and an interchangeable former of the required diameter bends it through the specified angle so the stretched surface can be inspected for defects. It is built for three-point bending with a former and handles root, face and side bends.

  • Two support rollers with pinned, adjustable spacing bars, so you can set l inside the d + 2 ts + 1 to d + 3.5 ts window for each specimen thickness.

  • Graduated base for fast, symmetric roller distance setting, which keeps the weld centred under the former.

  • Set of interchangeable formers in several thicknesses and radii, sized to specimen thickness, to cover d = 4 ts and the elongation-based formula.

  • Replaceable roller sleeves for different roller diameters.

  • Load capacity: 100 kN typical; higher capacities on request.

  • Material: hardened, corrosion-protected steel.

  • Machine connection: threaded spigot or pin adapter (clevis or threaded) to suit your load frame; compatible with electromechanical and servo-hydraulic universal test machines.

When you order, give us the specimen thickness and width, the former diameters you need, the roller diameter and your test machine connection. The fixture is designed around the former-and-rollers arrangement. If your procedure calls for the U-type plunger and die, the wrap-around roller method or a backing plate, tell us so we can discuss what fits. See the full range on our bend testing fixtures page and our bend testing application page.

Choosing a testing machine: how much force does a weld bend need?

This is where many labs get caught out. ISO 5173 does not state a force, so you have to estimate it. A quick engineering estimate (not part of the standard) uses the fully plastic bending moment of the specimen, Mp = σf × b × ts² / 4, where σf is a flow stress between yield and tensile strength. For three-point bending over a span l, the force to start plastic bending is about F = 4 Mp / l. The force often rises as the specimen wraps around the former and work-hardens, so allow a margin of at least 1.5 to 2 times the estimate.

  • 10 mm side bend, 25 mm plate, σf = 500 MPa: Mp = 500 × 25 × 10² / 4 = 312,500 N·mm. With d = 40 mm and l = 70 mm, F ≈ 4 × 312,500 / 70 ≈ 17.9 kN.

  • 20 mm full-thickness face bend, b = 4 ts = 80 mm: Mp = 500 × 80 × 20² / 4 = 4,000,000 N·mm. With d = 80 mm and l = 140 mm, F ≈ 16,000,000 / 140 ≈ 114 kN.

  • 30 mm full-thickness face bend, b = 120 mm: Mp = 500 × 120 × 30² / 4 = 13,500,000 N·mm. With d = 120 mm and l = 210 mm, F ≈ 54,000,000 / 210 ≈ 257 kN.

Mark-10 force testers are too small for ISO 5173. Even the largest Mark-10 F-series model, the F1505, tops out at 1,500 lbF (about 6.7 kN), well below the force for even a thin side bend. Use a Galdabini universal testing machine sized to your thickest specimen:

  • Side bends and thin plate: a Galdabini 100 kN benchtop UTM suits 10 mm side bends and reduced-thickness face and root bends, and matches the 100 kN typical rating of our fixture. A 50 kN benchtop can cover small side bends in lower-strength alloys.

  • Full-thickness face and root bends up to about 20 mm: a 200 kN or 250 kN floor-standing UTM, with a higher-capacity version of the fixture.

  • Thick plate (25 to 30 mm) and high-strength steels: a 600 kN floor-standing UTM, a 1,000 kN floor-standing frame or a Galdabini hydraulic UTM. Hydraulic frames also make sense if the same machine runs large transverse weld tensiles.

  • Stroke: check daylight and travel with the fixture installed; a 180° bend needs considerably more stroke than the specimen thickness.

Browse all floor-standing UTMs and benchtop UTMs.

Extensometers, deflectometers and other accessories

An extensometer is not needed for ISO 5173. The bend angle can be taken from former displacement (the method is in ISO 7438) or confirmed by the end-of-test condition, and bending elongation, when required, is measured from gauge marks before and after the test with a rule or calipers. A deflectometer is useful if you want a clean displacement record during the bend, but it is not a requirement of the standard. You do need good lighting for inspection and adapters that put the former and rollers on the load axis.

ISO 5173 test procedure step by step

  • 1. Confirm the application standard. Note the specimen types, number of specimens, bend angle and acceptance criteria it requires. ISO 15614-1, for example, typically calls for four transverse bends (two root and two face, or four side bends for thicker material).

  • 2. Extract and machine specimens. Remove material affected by thermal cutting, machine to thickness and width, remove weld reinforcement flush, round tension-face edges to r ≤ 0.2 ts (maximum 3 mm) and mark each specimen with its position.

  • 3. Measure. Record ts, b and Lt, and mark gauge length Lo centred on the weld if bending elongation is required.

  • 4. Calculate the former diameter. Use d = 4 ts when A ≥ 20 %, otherwise d = (100 × ts / A) − ts, using the lowest specified A of the materials joined.

  • 5. Set the rollers. Fit roller sleeves with R ≥ 20 mm and set the spacing within d + 2 ts + 1 ≤ l ≤ d + 3.5 ts using the graduated base, symmetric about the former axis.

  • 6. Position the specimen. Place the specimen with the surface to be examined facing away from the former, weld centre line under the former axis. Use a centring mark or etch to locate the weld.

  • 7. Bend. Apply load slowly and continuously at a constant speed. Stop at the angle in the application standard, or at about 180° when the former axis has passed between the roller axes.

  • 8. Remove and inspect. Examine the outer surface and both sides for cracks and other imperfections, measure the largest opening, and note whether defects start at the specimen corners.

  • 9. Report. Record the items listed below and judge the result against the application standard.

Calculations with a worked example

Example 1: side bend in carbon steel

  • Parent plate 25 mm, minimum specified elongation A = 22 %. Side bend specimen ts = 10 mm, b = 25 mm.

  • Former: A ≥ 20 %, so d = 4 × 10 = 40 mm.

  • Roller spacing: l from 40 + 2 × 10 + 1 = 61 mm to 40 + 3.5 × 10 = 75 mm. Set l = 70 mm.

  • Specimen length: with R = 25 mm rollers, Lt ≥ 70 + 2 × 25 = 120 mm.

Example 2: lower-elongation parent metal

  • Parent material with A = 16 %, ts = 10 mm.

  • Former: d = (100 × 10 / 16) − 10 = 62.5 − 10 = 52.5 mm.

  • Roller spacing: l from 52.5 + 20 + 1 = 73.5 mm to 52.5 + 35 = 87.5 mm. Set l = 80 mm.

  • Specimen length: with R = 25 mm, Lt ≥ 80 + 50 = 130 mm.

Example 3: bending elongation

If the application standard asks for bending elongation, ISO 5173 gives the gauge length Lo to use: for fusion welds Lo = Ls, 2 Ls or Ls − ts depending on the case, and for pressure, electron beam and laser welds Lo = ts or 2 ts, centred on the former axis. Elongation is the increase in gauge length divided by Lo. With Ls = 16 mm and Lo = Ls = 16 mm marked on the tension face, a measured length after bending of 22.4 mm gives (22.4 − 16) / 16 × 100 = 40 %.

Typical results and what to report

A good weld bends to the full angle with a smooth stretched surface. A failing weld shows open lack of fusion along the fusion line, root defects, slag lines or cracks. ISO 5173 does not judge the result: the application standard does. ISO 15614-1, for example, does not allow imperfections larger than 3 mm in any direction on bend specimens, with indications at the specimen corners disregarded; check the current edition of your application standard for exact wording. ISO 5173 lists these report items:

  • Reference to ISO 5173:2023.

  • Specimen identification, parent material and any heat treatment, including hydrogen-removal treatment.

  • Specimen shape and dimensions, and the bend type with its code (TFBB, TRBB, TSBB and so on).

  • Test conditions: method, former or roller diameter, roller spacing and radius, and whether a U-type jig was used.

  • Test temperature, test speed if known, and bending angle.

  • Bending elongation and gauge length, if applicable.

  • Type and size of imperfections found.

  • Application standard, deviations from the procedure, unusual features, test date and result.

Common errors in ISO 5173 bend testing

  • Using the mill certificate elongation instead of the specified minimum A, which gives a former that is too small or too large.

  • Roller spacing outside the window. Too tight and the specimen jams or is sheared at the rollers; too wide and the bend is not guided tightly around the former.

  • Weld off-centre. The strain concentrates in the HAZ or parent metal instead of the weld. Etch to locate the weld if it is not visible.

  • Sharp or scratched edges. Corner cracks from poor edge preparation fail good welds. Round to r ≤ 0.2 ts, maximum 3 mm, without transverse marks.

  • Leaving weld reinforcement on, which concentrates strain at the toes.

  • Underestimating force. Thick full-thickness face and root bends often need a floor-standing frame; a stalled machine leaves an incomplete bend.

  • Ignoring strain localisation in mismatched joints. Where parent, HAZ and weld metal differ strongly, the standard points to roller, backing plate or longitudinal bends instead.

ISO 5173 vs ASTM E190, ASTM E290 and related standards

  • ASTM E190: the US guided bend test for ductility of welds. Like ISO 5173 it bends a weld specimen around a plunger or mandrel and inspects the convex surface, but specimen dimensions, jig geometry and terminology differ, so you cannot simply swap one for the other in a qualification.

  • ASTM E290: bend testing of material for ductility, covering guided, free and semi-guided bends on plain metal rather than welds.

  • ISO 7438: the ISO bend test for metallic materials (not welds); ISO 5173 refers to it for calculating bend angle from displacement.

  • ISO 15614-1, ISO 15614-2 and ISO 9606-1: the application standards that call up ISO 5173 and set the number of specimens, bend angle and acceptance criteria.

  • Other weld tests: ISO 4136 (transverse tensile), ISO 9016 (impact) and ISO 17639 (macro examination) usually run on the same test piece; ASME Section IX and AWS use their own bend jigs. For parent metal tensiles see ISO 6892-1 and ASTM A370.

Equipment summary

ISO 5173 FAQ

What is ISO 5173?

ISO 5173 is the ISO test method for destructive bend tests on welds in metallic materials. It covers transverse root, face and side bends, longitudinal bends and cladding bends, and defines specimen dimensions, former diameters, roller spacing and reporting. The current edition is ISO 5173:2023.

What is the latest edition of ISO 5173?

ISO 5173:2023, the fourth edition. It replaces ISO 5173:2009 and its 2011 amendment, adds guided roller and longitudinal bend tests for heterogeneous joints, and corrects figures.

How do I calculate the former diameter in ISO 5173?

For steel, nickel and nickel alloys with a minimum specified elongation A of 20 % or more, d = 4 ts. For lower elongation, d = (100 × ts / A) − ts. Aluminium uses the same formula above 5 % elongation; at 5 % or less the specimen is annealed first.

What roller spacing does ISO 5173 require?

For the former method the distance between rollers is d + 2 ts + 1 ≤ l ≤ d + 3.5 ts in millimetres, and the roller radius is at least 20 mm. With a backing plate, add its thickness to ts in both limits.

What bend angle is used?

The angle set by the application standard. If none is given, specimens are bent to about 180°, which for the former method is reached when the former axis passes between the roller axes.

What is the specimen thickness for a side bend?

Side bend specimens are machined to 10 ± 0.5 mm thick, and their width equals the parent thickness. Joints thicker than 40 mm may be split into several side bend specimens.

What test speed does ISO 5173 specify?

No numerical speed. Load should be applied slowly and continuously, kept constant where possible, and recorded in the report when known.

What are the acceptance criteria for an ISO 5173 bend test?

ISO 5173 has none. The application standard sets them. ISO 15614-1, for example, does not allow imperfections larger than 3 mm in any direction; check the current edition of your application standard.

How much force does a weld bend test need?

It depends on thickness, width and strength. A 10 mm steel side bend may need around 20 kN, a full-thickness face bend in 20 mm steel plate over 100 kN, and 30 mm plate over 250 kN. Size the machine with a margin of 1.5 to 2 times your estimate.

Can I run ISO 5173 on a Mark-10 force tester?

No. The largest Mark-10 F-series tester is rated at about 6.7 kN, far below the force for even a thin weld bend. Use a Galdabini universal testing machine from 100 kN benchtop upward.

Is ISO 5173 the same as ASTM E190?

They test the same thing, the ductility and soundness of a weld in bending, but specimen dimensions, jig geometry and terminology differ. Follow whichever standard your qualification code calls for.

Do I need an extensometer for ISO 5173?

No. Bend angle comes from former displacement or the end-of-test condition, and bending elongation, if required, is measured from gauge marks before and after the test.

Need a fixture, grips or a complete test system for ISO 5173? Contact Universal Grip with your material, specimen size and machine connection and we will quote the right setup.

bottom of page