ISO 8295 is the international method for measuring the static and dynamic coefficients of friction (COF) of plastic film and sheeting, sliding against itself or against another material such as metal, paper or board. A sled of defined mass and contact area presses two surfaces together, one surface is drawn across the other at constant speed, and the starting and sliding forces are divided by the normal force to give two dimensionless numbers: µs and µd.
Film producers, converters, laminators and packaging engineers use it to control slip and anti-block additives and to make sure film runs smoothly on form-fill-seal, wrapping and bag-making lines. This guide covers the current edition, specimens, apparatus, the step-by-step procedure, a worked calculation, common errors and how ISO 8295 differs from ASTM D1894. Universal Grip makes a horizontal-plane friction fixture for ISO 8295 that mounts on a universal testing machine; details are in the equipment section.
In this guide: What ISO 8295 Measures · Current Edition, Scope and Adoptions · Test Specimens and Conditioning · Apparatus: Table, Sled, Drive and Force Measurement · ISO 8295 Test Procedure Step by Step · Calculation and Worked Example · Reading the Force Trace · What Drives Film COF: Additives, Age, Surface and Counterface · Common Errors and Sources of Scatter · ISO 8295 vs ASTM D1894 and Related Standards · ISO 8295 Equipment from Universal Grip · FAQ
What ISO 8295 Measures
Friction is the resistance two surfaces in contact build up against sliding. ISO 8295 splits it into two values:
-
Static (starting) friction, Fs: the threshold force that must be overcome to start sliding. It appears as the first peak on the force trace.
-
Dynamic (sliding) friction, Fd: the force needed to keep the surfaces sliding at the test speed, taken as the average force during steady sliding.
-
Normal force, Fp: the force pressing the surfaces together, set by the sled mass (1.96 N for the 200 g sled).
-
Coefficients: µs = Fs / Fp and µd = Fd / Fp. Both are dimensionless.
Static COF is usually higher than dynamic COF. A low dynamic value means film slides easily over itself or over forming collars and guides; a very low static value can make stacked bags or rolls slide apart. Most packaging specifications set a range for both.
The standard is explicit that it serves primarily for quality control. It does not give a comprehensive assessment of how film will run on a packaging or processing machine, because electrostatic charge, air cushions between layers, temperature rise and abrasion also affect real-world behavior.
Current Edition, Scope and Adoptions
The current version is ISO 8295:1995, the second edition, prepared by ISO/TC 61/SC 11. It replaced ISO 8295:1986. Despite its age, the standard is current: ISO most recently reviewed and confirmed it in 2026, and no revision is under way. It is adopted in Europe as EN ISO 8295 (BS EN ISO 8295, DIN EN ISO 8295); the older German film friction method, DIN 53375, has been withdrawn.
Scope
-
Plastic film and sheeting sliding over itself or over other substances
-
Non-sticky film and sheeting up to approximately 0.5 mm thick (the standard calls all of it "film")
-
Not intended for tacky or self-adhesive films such as cling film, which block rather than slide
Two cautions are written into the scope. First, static friction generally increases with the time the surfaces stay in contact before sliding, so the standard fixes the contact time to make results comparable. Second, slip additives can migrate (bloom) to the surface or exude over time, so COF changes as film ages. Always relate results to the film's age and record it.
Test Specimens and Conditioning
-
Specimen size: two specimens of about 80 mm × 200 mm for each measurement
-
Number: at least three pairs, taken from points spread evenly across the film width (or around the circumference of tubular film)
-
Direction: long axis parallel to the machine direction unless otherwise specified
-
Surfaces: if the two faces of the film behave differently, identify them as side 1 and side 2 and test the combinations agreed (1/1, 2/2 and/or 1/2)
-
Film against another material: the lower film specimen is replaced by the counterface material, for example a metal sheet, paper or board
Three pairs is a minimum. ISO 8295 notes that more may be needed to estimate a statistical tolerance interval, referring to ISO 2602 for guidance, so many labs test five or more.
Handling
Friction is a surface property, and a fingerprint, a trace of skin oil or a dusty bench is enough to change it. Wear clean gloves, touch only the specimen edges, never wipe the test surface, and keep specimens face-to-face or covered until testing. Do not fold or crease film in the contact area.
Conditioning
Condition specimens for at least 16 h in the 23/50 standard atmosphere of ISO 291 (23 °C, 50 % relative humidity) unless another condition is specified, and test in the same atmosphere. Slip additive performance is temperature sensitive, so a warm lab can produce noticeably different results from a 23 °C lab on the same film.
Apparatus: Table, Sled, Drive and Force Measurement
Test table
A horizontal, flat, smooth table made of non-ferromagnetic metal. The lower specimen is fixed to it with double-sided tape or a clamp so it lies flat without wrinkles.
Sled
-
Contact area: square, 40 cm² (63 mm × 63 mm)
-
Total mass: 200 g ± 2 g, giving a normal force of 1.96 N ± 0.02 N
-
Base: covered with an elastic material such as felt, to spread the pressure evenly; it should be fine enough not to emboss thin films
Drive and speed
The relative motion must be free of vibration at 100 mm/min ± 10 mm/min. For special films, or where difficulties arise at the normal speed, 500 mm/min ± 10 mm/min may be used, and the speed must then be stated in the test report. Either the table or the sled may be the moving element. The standard illustrates a moving-table instrument, and it also allows a tensile testing machine to be used with a pulley that turns the vertical crosshead motion into a horizontal pull.
Force measurement
-
Force measuring error: not more than ±2 %
-
Response: transition time t90 of no more than 0.5 s, so the system can follow the static peak
-
Alignment: the pulling direction must be in straight alignment with the plane of friction; a pull angled up or down changes the effective normal force
Forces are small. With a 1.96 N normal force and typical film COF between about 0.1 and 0.6, friction forces fall roughly between 0.2 N and 1.2 N. Choose a low-capacity load cell whose accuracy class holds at that level, and a data rate high enough to catch the static peak.
The spring (friction drag) rule
This is the detail most guides leave out. For measuring static friction, ISO 8295 specifies that the connection between the moving specimen and the load cell has a stiffness of 2 N/cm ± 1 N/cm, for example a suitable spring. The controlled compliance lets force build smoothly so a clean, repeatable starting peak forms. For dynamic friction on films that show stick-slip, the spring is replaced with a rigid connection, because a spring would amplify the stick-slip oscillation and distort the sliding average.
ISO 8295 Test Procedure Step by Step
The sequence below follows the film-against-film procedure. In the standard's own arrangement, the upper film specimen is connected to the load cell and the sled rests on top of it; many fixtures instead carry the upper specimen on the sled face. Both put the two films in contact under the sled's 40 cm² footprint and 1.96 N load. Use the arrangement your specification calls for.
-
1. Condition the specimens for at least 16 h at 23 °C / 50 % RH and work in that atmosphere.
-
2. Fix the first specimen flat to the table with double-sided tape or a clamp, aligned with the direction of travel, test surface up.
-
3. Prepare the second specimen. In the standard arrangement its leading end is reinforced with a small plate of no more than 5 g and connected to the load cell through the spring (for static friction) or a rigid link.
-
4. Lay the second specimen on the first with the agreed surfaces facing each other.
-
5. Place the sled gently and without shock in the middle of the contact area. Dropping it raises static friction.
-
6. Wait 15 s with the surfaces in contact and at rest, then start the drive. The fixed contact time is what makes static values comparable between tests and labs.
-
7. Record force against displacement. The first maximum of the rising force is the static friction force Fs.
-
8. Continue sliding for at least 6 cm and take the average force over that distance, excluding the static peak, as the dynamic friction force Fd.
-
9. Use fresh specimens for every measurement; a sliding surface is altered by the test.
-
10. Repeat for at least three pairs and report the mean values.
Note: For high-blocking films, ISO 8295 advises reducing the upper specimen as closely as possible to the sled area so that only the loaded area is in contact.
Calculation and Worked Example
µs = Fs / Fp and µd = Fd / Fp, where Fp is the normal force from the sled (200 g × 9.81 m/s² = 1.96 N).
Worked example: LDPE film against itself, 100 mm/min
-
Normal force: Fp = 0.200 kg × 9.81 m/s² = 1.962 N, rounded to 1.96 N
-
Pair 1: Fs = 0.52 N, Fd (average over 6 cm) = 0.41 N
-
µs = 0.52 ÷ 1.96 = 0.265, reported as 0.27
-
µd = 0.41 ÷ 1.96 = 0.209, reported as 0.21
-
Pair 2: Fs = 0.49 N gives µs = 0.25; Fd = 0.40 N gives µd = 0.20
-
Pair 3: Fs = 0.51 N gives µs = 0.26; Fd = 0.42 N gives µd = 0.21
-
Means of three pairs (using unrounded values): µs = 0.26, µd = 0.21
Report coefficients to two decimal places. Three significant figures overstate the precision of a test this sensitive to surface condition.
Sled inertia
When the sled is pulled from rest, its inertia adds a little force at the start of motion, so the measured starting coefficient overshoots the true value. ISO 8295 quantifies the effect as an overshoot of about 0.005 in the coefficient, which is a 2.5 % error at a coefficient of 0.2. It matters most for low-slip films, and it is one more reason to keep sled mass, spring and speed exactly as specified when comparing results.
Reading the Force Trace
A typical ISO 8295 trace rises as the connection loads up, peaks when the surfaces break loose (static friction), drops, and then settles into a band during sliding (dynamic friction). Common patterns:
-
Clear peak then steady plateau: the normal case. Read Fs at the peak and Fd as the plateau average.
-
No distinct peak: static and dynamic friction are about equal, so no separate starting value can be picked out. State this in the report rather than forcing a static value from noise.
-
Saw-tooth trace (stick-slip): the surfaces alternately stick and release. Switch to a rigid connection for the dynamic value and report that stick-slip occurred; the average still gives µd, but the amplitude is useful information.
-
Force rising steadily during sliding: often a sign of blocking, additive transfer, film wrinkling ahead of the sled or electrostatic attraction.
-
Very high, erratic values: suspect surface contamination, damaged film or a wrong surface pairing.
What Drives Film COF: Additives, Age, Surface and Counterface
Interpreting an ISO 8295 result means knowing what moves it. The usual drivers in packaging film are:
-
Slip additives: fatty acid amides such as erucamide and oleamide are added to polyolefin films to lower COF. They work by migrating to the surface, which takes time, so COF typically falls over the first days after extrusion and then levels off. This is why ISO 8295 asks you to relate results to film age.
-
Anti-block additives: fine mineral particles roughen the surface slightly and stop layers sticking together on the roll, which mainly lowers static friction and blocking.
-
Surface treatment and coatings: corona or flame treatment, print, varnish and coatings change surface energy and roughness, so treated and untreated sides often give different values. That is why the standard has you identify side 1 and side 2.
-
Counterface: film-to-film COF and film-to-metal COF are different properties. A film that slides well on itself can still drag on a stainless forming collar, so test the pairing that matters on your line.
-
Temperature and lamination: additives can migrate into adhesive layers in laminates, and warm conditions change additive behavior, so laminate COF can drift after curing or storage.
For QC trending, test at a fixed film age, on the same surface pairing, with the same sled backing and connection. For troubleshooting a line, add tests against the actual machine contact material. Off-standard conditions, such as testing at line temperature in an environmental chamber, are useful for engineering, but report them as deviations from ISO 8295.
Common Errors and Sources of Scatter
-
Wrong formula: the coefficients divide friction force by normal force. Dividing static force by dynamic force, which appears on some published pages, does not give a coefficient of friction.
-
Contact time not controlled: static friction rises with dwell time. Hold the 15 s wait every time.
-
Sled dropped or slid into position: place it gently in the middle of the contact area.
-
Pull not horizontal: a pulley or hook set above or below the friction plane adds or removes normal force.
-
Spring or link wrong for the measurement: use the specified 2 N/cm compliance for static friction and a rigid link for stick-slip dynamic measurement.
-
Contaminated or reused specimens: use fresh, untouched specimens for every measurement.
-
Film age ignored: slip additives keep migrating for days after extrusion. Record the production date and test at a consistent age for QC trending.
-
Load cell too large: friction forces are often under 1 N. An oversized cell or a low data rate will flatten the static peak.
-
Temperature drift: test in the conditioned atmosphere; friction of slip-modified films can shift with a few degrees.
ISO 8295 vs ASTM D1894 and Related Standards
ASTM D1894 is the North American counterpart and measures the same static and kinetic coefficients with a sled on a horizontal plane. The principle and the 200 g sled mass are common to both, but results are not interchangeable:
-
Speed: ISO 8295 runs at 100 mm/min (or 500 mm/min); ASTM D1894 runs at 150 mm/min ± 30 mm/min.
-
Specimens: ISO uses pairs of about 80 mm × 200 mm; ASTM uses a 250 mm × 130 mm plane specimen and a sled specimen of about 120 mm square that wraps the sled.
-
Sliding distance for the kinetic average: about 6 cm in ISO 8295; about 130 mm of travel in ASTM D1894.
-
Minimum number: three pairs in ISO 8295; ASTM D1894 calls for five valid results.
-
Contact time and connection: ISO fixes a 15 s dwell and specifies the 2 N/cm spring rule for static measurement; ASTM has its own setup requirements.
-
Conditioning: ISO 291 (23/50, at least 16 h); ASTM D618.
Report which standard you used; a specification written around one cannot be checked with the other.
Related standards
-
ISO 291: standard atmospheres for conditioning and testing plastics
-
ISO 2602: statistical interpretation of test results, referenced for the number of specimens
-
JIS K 7125: the Japanese film friction method
-
Film tensile properties on the same machine: ISO 527-3 and ASTM D882
Browse every method we cover on our ISO standards page.
ISO 8295 Equipment from Universal Grip
Universal Grip's ISO 8295 Friction Test Fixture (part ref. UGC-ISO8295-FTF) is a horizontal-plane fixture for measuring the static and kinetic coefficients of friction of plastic film and sheeting on an electromechanical universal testing machine. A weighted sled carrying one film specimen is drawn across a second specimen clamped to the table, via a low-friction pulley and wire connected to the load cell on the rising crosshead.
-
Test method: static and kinetic coefficient of friction, per ISO 8295
-
Loading: horizontal sliding via pulley, tension from the crosshead
-
Specimens: film or sheet, one on the sled and one on the table
-
Sled: to ISO 8295 mass and contact area, with felt or elastomer backing; interchangeable sleds
-
Table: knob-clamped table plate holds the base film flat
-
Load capacity: low force; 10–50 N load cell recommended
-
Materials: anodised aluminium and stainless steel
-
Machine connection: base adapter to suit your frame; wire hook to the load cell
-
Compatible frames: electromechanical universal test machines
The felt-backed sled follows the elastic covering described in ISO 8295; the elastomer-backed sled gives you a second option for labs that also run ASTM-style setups. Because the fixture uses your existing frame, a single-column benchtop universal testing machine with a low-force load cell is all that is needed. Testing software that records force against displacement lets you pick the static peak and average the dynamic band automatically.
When ordering, specify film or sheet thickness, sled backing material, test machine base and load cell connection, including any spring or rigid-link requirement your procedure calls for. Explore our plastics testing range, related accessories and adapters, or contact us for a quote.
ISO 8295 FAQ
What is the current edition of ISO 8295?
The current edition is ISO 8295:1995, the second edition. ISO reviewed and confirmed it in 2026, so it remains current, and no newer version is in development. It is adopted in Europe as EN ISO 8295.
What is the difference between static and dynamic coefficient of friction?
The static coefficient (µs) is the force needed to start sliding divided by the normal force; it comes from the first peak on the force trace. The dynamic coefficient (µd) is the average force needed to keep sliding divided by the normal force. Static is usually higher than dynamic.
What sled is used in ISO 8295?
The sled has a square contact area of 40 cm² (63 mm × 63 mm) and a total mass of 200 g ± 2 g, giving a normal force of 1.96 N. Its base is covered with an elastic material such as felt so pressure is even across the film.
What test speed does ISO 8295 use?
The standard speed is 100 mm/min ± 10 mm/min. For special films or where problems arise, 500 mm/min ± 10 mm/min may be used, and the speed must then be stated in the test report.
How do you calculate coefficient of friction per ISO 8295?
Divide the friction force by the normal force: µs = Fs / Fp and µd = Fd / Fp. With a 200 g sled, Fp = 1.96 N, so a static peak of 0.52 N gives µs = 0.27 and an average sliding force of 0.41 N gives µd = 0.21. Do not divide static force by dynamic force; that ratio is not a coefficient of friction.
How many specimens does ISO 8295 require?
At least three pairs of specimens, each about 80 mm × 200 mm, taken from points spread across the film width. The standard notes that three is a minimum and more may be needed for a reliable statistical estimate.
Why does ISO 8295 specify a 15 second wait before sliding?
Static friction increases with the time two surfaces stay in contact. Fixing the dwell at 15 s makes static results comparable between tests, operators and labs. Changing the wait time changes µs.
Does ISO 8295 require a spring between the sled and the load cell?
For static friction, the standard specifies a connection stiffness of 2 N/cm ± 1 N/cm, for example a suitable spring, so a clean starting peak forms. For dynamic friction on films that show stick-slip, the spring is replaced with a rigid connection so it does not amplify the oscillation.
Is ISO 8295 the same as ASTM D1894?
No. Both use a 200 g sled on a horizontal plane, but ASTM D1894 runs at 150 mm/min, uses larger specimens and a longer sliding distance, and has different minimum specimen numbers. Results are related but not interchangeable; see our ASTM D1894 guide.
What thickness of film is covered by ISO 8295?
ISO 8295 covers non-sticky plastic film and sheeting up to approximately 0.5 mm thick. Tacky or self-adhesive films are outside the scope because they block rather than slide.
Can ISO 8295 measure film against metal or paper?
Yes. The standard covers film sliding over itself or over other substances. The lower film specimen is replaced by the counterface material, such as a metal sheet, paper or board, and the test is otherwise run the same way.
Can I run ISO 8295 on a universal testing machine?
Yes. ISO 8295 allows a tensile testing machine with a pulley that turns vertical crosshead travel into a horizontal pull. Universal Grip's friction fixture works this way on electromechanical frames, with a 10–50 N load cell recommended. Contact us for a quote.
Need a fixture, grips or a complete test system for ISO 8295? Contact Universal Grip with your material, specimen size and machine connection and we will quote the right setup.