ISO 8339
Tensile Properties of Building Sealants (Extension to Break)

Downloads: ISO 8339 Sealant Tensile Test Fixture (H-Block) – Universal Grip Data Sheet (PDF)
Written by Chris Thomas, Universal Grip Company · Reviewed by Frank Bertini · Updated October 31, 2026
ISO 8339 is the international test method for determining the tensile properties of building construction sealants by stretching an H-block specimen to break. A bead of sealant, 12 mm wide, 12 mm deep and 50 mm long, is cured between two parallel substrates of mortar, anodized aluminium or glass, then pulled apart at a slow constant rate while force and extension are recorded until the bead fails. The results, secant tensile modulus, elongation at break and failure mode, are what sealant manufacturers, façade and glazing consultants, certification bodies and QC laboratories use to classify a sealant as low modulus or high modulus under ISO 11600 and to support CE marking declarations in Europe. This guide explains the method clause by clause, gives a worked calculation, lists the common mistakes, and shows how to set the test up with the Universal Grip ISO 8339 H-block fixture.
ISO 8339 at a glance
-
Current edition: ISO 8339:2005 (second edition), last reviewed and confirmed by ISO in 2020. ISO has a third edition in development (ISO/DIS 8339, retitled *Building and civil engineering sealants — Determination of tensile properties (Extension to break)*). Check whether it has been published before you write a new procedure.
-
Scope: tensile properties of sealants used in joints in building construction. Tensile properties at *maintained* extension are covered separately in ISO 8340.
-
Specimen: H-block with a sealant bead of 12 mm × 12 mm × 50 mm bonded between two substrates of the same material, formed with 12 mm × 12 mm anti-adherent spacers.
-
Substrates: mortar, anodized aluminium and/or glass, as specified in ISO 13640.
-
Number of specimens: three for each substrate type and each test temperature.
-
Conditioning: Method A (28 days at 23 ± 2 °C and 50 ± 5 % RH) or Method B (Method A followed by three oven/water cycles), chosen by agreement.
-
Test temperatures: 23 °C and −20 ± 2 °C. Specimens for the cold test are held at −20 °C for at least 4 h first.
-
Rate of extension: 5.5 ± 0.7 mm/min, continued to rupture.
-
Results: secant tensile modulus in N/mm² (to 0.01) at 100 %, 60 % or an agreed elongation; elongation at break in % (to the nearest 5 %); and the type of failure, adhesive and/or cohesive.
-
Related standards: ISO 8340, ISO 11600, ISO 9046, ISO 9047, ISO 7389, ISO 10590, ISO 13640, ISO 6927, EN ISO 8339.
What ISO 8339 measures and who uses it
A building joint sealant has to stretch and compress as panels, frames and glass move with temperature, wind and settlement. If the sealant is too stiff, it pulls hard on the joint faces and can tear away from a weak substrate such as mortar or render. If it is too weak, it fails cohesively in the bead. ISO 8339 gives a standard way to put a number on that behaviour.
The main result is the secant tensile modulus. This is the stress at a chosen elongation, calculated as force at that elongation divided by the initial cross-section. It is a secant value, a straight line from the origin to a point on the curve, not the slope of the curve. It is normally quoted at 100 % elongation, the bead stretched to twice its original 12 mm width, or at 60 %. The other results are elongation at break, how far the bead stretched before it ruptured, and the failure mode: cohesive (the sealant tore within itself), adhesive (it peeled from a substrate face) or a mix of both.
These results are used by:
-
Sealant manufacturers: to develop formulations, check batches and support declarations of performance.
-
Classification and certification laboratories: ISO 11600 splits class 25 and class 20 sealants into low modulus (LM) and high modulus (HM) using the secant modulus at +23 °C and −20 °C.
-
Façade, curtain-wall and glazing engineers: to choose sealants that will not overload weak joint faces or lose adhesion on aluminium and glass.
-
Primer and substrate suppliers: to show adhesion on specific mortars, anodized finishes and glass.
ISO 8339 specimens: dimensions, substrates and preparation
Every ISO 8339 specimen has the same sealant geometry: a bead 12 mm × 12 mm in section and 50 mm long, bonded on its two 12 mm × 50 mm faces to a pair of parallel substrates. The bonded area on each face, and therefore the cross-section used in the modulus calculation, is 12 × 50 = 600 mm². Two removable spacers, each 12 mm × 12 mm with an anti-adherent surface, sit at the ends of the cavity and set the 12 mm joint width. A sheet of anti-adherent material such as polyethylene film, preferably the one the sealant manufacturer recommends, closes the base of the cavity during filling.
Substrates are mortar, anodized aluminium or glass, with materials specified in ISO 13640. The standard's figures give the substrate dimensions. Glass and aluminium substrates are commonly 75 mm × 12 mm × 6 mm bars, and mortar blocks are thicker. The 2005 edition allows other substrate sizes as long as the sealant bead and bonded area match the figures. That matters when you order holders, because the holder has to fit the outside of the block you actually use.
Preparing the H-blocks
-
Bring the sealant, substrates and spacers to 23 ± 2 °C before assembly.
-
Clean the substrates and apply primer only if the sealant manufacturer specifies one. Record the primer used.
-
Mix multi-component sealants as the manufacturer instructs.
-
Fill the cavity without trapping air. Press the sealant firmly against both substrate faces so it wets them fully.
-
Tool the sealant flush with the faces of the substrates and spacers.
-
Leave the spacers in place throughout conditioning. They hold the joint at exactly 12 mm while the sealant cures.
-
Prepare three specimens for each substrate type and each test temperature.
Conditioning: Method A and Method B
Cure has a large effect on modulus, so ISO 8339 fixes the conditioning. The parties choose one of two methods.
-
Method A: 28 days at 23 ± 2 °C and 50 ± 5 % relative humidity.
-
Method B: Method A first, then three repeats of this cycle: 3 days in a ventilated oven at 70 ± 2 °C, 1 day immersed in distilled water at 23 °C, 2 days in the oven at 70 °C, and 1 day in distilled water at 23 °C. The order oven–water–oven–water may start at the second pair instead. After the last cycle, specimens are stored for 24 h at 23 °C and 50 % RH before testing.
Method B accelerates and completes cure, and it exposes the bond to heat and water. The standard itself notes that Method B is not suitable for judging durability, so do not present Method B results as an ageing or weathering study. Plan the calendar: Method A takes four weeks, and Method B adds three more weeks plus a day.
Test speed, temperature and machine requirements
ISO 8339 requires a tensile testing machine that can extend the specimen at 5.5 ± 0.7 mm/min and record a force/extension diagram. That is slow. At 5.5 mm/min a bead reaching 400 % elongation, 48 mm of extension, takes almost nine minutes, so the frame must hold a steady low speed for a long time. For the cold test you also need a refrigerated enclosure that holds the specimen at −20 ± 2 °C while it is being extended, not just a freezer to store it in.
Forces are modest but not trivial. With a 600 mm² cross-section, every 0.1 N/mm² of stress is 60 N of force. A low-modulus sealant at the ISO 11600 limit of 0.4 N/mm² at 100 % pulls about 240 N at 23 °C. At the −20 °C limit of 0.6 N/mm² that becomes about 360 N. High-modulus and structural sealants can be several times higher, and the peak force at break is often higher than the force at 100 %. Estimate the worst case as expected stress × 600 mm² and pick a load cell with comfortable headroom.
The Universal Grip ISO 8339 H-block fixture
Our ISO 8339 Sealant Tensile Test Fixture (H-Block), part ref. UGC-ISO8339-TF, is a pair of open-frame specimen holders built for tensile testing of sealant H-blocks to break. Each holder slides over one substrate block, so the test machine pulls the sealant bead in uniform tension at a constant rate while force and extension are recorded until cohesive or adhesive failure.
-
Open window-frame holders slide over the substrate blocks. No adhesive and no screws are needed, so specimens load quickly and the substrates are not damaged.
-
Even load across the full substrate width. The frame bears on the back face of each substrate, which keeps the bead in uniform tension instead of peeling it from one end.
-
Self-aligning swivel connections reduce bending on the sealant joint.
-
Suits mortar, glass and aluminium substrates of standard H-block size.
-
Load capacity: 1 kN standard, with higher capacities on request.
-
Material: aluminium alloy or stainless steel.
-
Machine connection: clevis pin or threaded adapter to suit your frame. Adapters are supplied, and we stock more adapters for other frames.
-
Compatible frames: electromechanical universal test machines.
When you order, tell us your substrate block dimensions, substrate material, required capacity and the connection on your test machine. That matters most if you use non-standard substrates, which the 2005 edition allows. See our tensile grips range and our adhesives testing page for related fixtures, or contact us to confirm a configuration. As with any data sheet, specifications are typical and are confirmed at time of quote.
Choosing a testing machine for ISO 8339
Mark-10 motorized testers for QC and 23 °C work
For batch QC at 23 °C a Mark-10 F-series tester fits the force range well, but check the speed. The standard speed range of the F105, F305 and F505 is 13–330 mm/min. That does not reach 5.5 mm/min, so you need the low-speed option, which extends the range down to 0.5 mm/min. With that option fitted:
-
The F305 (300 lbF, about 1.3 kN) suits most low- and high-modulus building sealants and matches the fixture's 1 kN standard rating.
-
The F505 (500 lbF, about 2.2 kN) gives extra headroom for stiff or structural products when the fixture is ordered at a higher capacity.
-
The F105 (100 lbF, about 450 N) covers low-modulus sealants at 23 °C, but it is tight for high-modulus products and for −20 °C testing. We would not recommend it as the only frame for a full ISO 11600 program.
All three have 457 mm of travel, far more than an H-block needs, ±0.2 % speed accuracy and 5,000 Hz sampling, which captures the break cleanly. Browse all tensile testers.
Galdabini universal testing machines for −20 °C and certification work
The −20 °C half of ISO 8339 is where a full universal testing machine earns its place. A Galdabini 2.5 kN or 5 kN benchtop UTM with an environmental chamber (−80 to +280 °C) holds the specimen at −20 ± 2 °C during extension, as the standard requires. It runs the slow constant rate, records the full force/extension diagram, and calculates secant modulus at 60 % or 100 % automatically in software. See all benchtop universal testing machines.
Do you need an extensometer?
Usually not. ISO 8339 defines elongation from the change in joint width, and the substrates, holders and frame are far stiffer than the sealant, so crosshead displacement is a good measure of bead extension at these forces. Zero the displacement with the spacers removed and the specimen just seated. A video extensometer is a genuine help in two cases: research work where you want the true gap between the substrate faces, and cold testing inside a chamber, where a non-contact system can measure through the window without touching a soft, sticky bead. Clip-on extensometers are not practical on an H-block.
ISO 8339 test procedure, step by step
-
Check conditioning. Confirm Method A or B was completed and record which one. Method B specimens need their 24 h at 23 °C and 50 % RH after the last cycle.
-
Inspect each specimen. Look for voids, poor tooling, substrate cracks or a bead that has sagged. Measure the bead width and length if your quality system requires it. Use 12 mm and 600 mm² unless the measured values differ meaningfully.
-
Fit the fixture. Mount the two holders on the frame with the swivel connections free and the holder centrelines in line. Set the gap so the specimen can be dropped in without loading it.
-
For −20 °C tests: store the specimens at −20 ± 2 °C for at least 4 h, and pre-cool the holders inside the chamber. Load quickly and let the chamber recover before you start.
-
Load the specimen. Slide each substrate into its holder so the frames bear evenly on the back faces. Check that the bead is vertical and centred.
-
Remove the spacers. This is the most commonly missed step. If the spacers stay in, you are testing them, not the sealant.
-
Zero force and displacement with the specimen seated but unloaded.
-
Extend at 5.5 ± 0.7 mm/min to rupture, recording force against extension continuously.
-
Record the failure mode for each specimen: adhesive (from which substrate), cohesive, or mixed, with an estimate of the proportion.
-
Repeat for the other two specimens in the set, then for each substrate and temperature.
Calculations with a worked example
ISO 8339 uses two simple formulas.
-
Secant tensile modulus: σ = F / s, where F is the force (N) at the chosen elongation and s is the initial cross-section (mm²). Report each value to 0.01 N/mm².
-
Elongation at break: E = (W₁ − W₀) / W₀ × 100, where W₀ is the original joint width (12 mm) and W₁ is the width at break. Report to the nearest 5 %.
Worked example. A one-part sealant is tested on anodized aluminium after Method A conditioning. The cross-section is 12 mm × 50 mm = 600 mm². 100 % elongation is reached when the joint has opened by 12 mm, to 24 mm.
-
23 °C, force at 100 % elongation: 216 N, 222 N and 210 N. Modulus = 216/600 = 0.36, 222/600 = 0.37 and 210/600 = 0.35 N/mm². Mean = 0.36 N/mm².
-
−20 °C, force at 100 % elongation: 318 N, 330 N and 324 N. Modulus = 0.53, 0.55 and 0.54 N/mm². Mean = 0.54 N/mm².
-
23 °C, extension at break: 40.8 mm, 43.1 mm and 38.9 mm. Elongation at break = 40.8/12 × 100 = 340 %, 43.1/12 × 100 = 359.2 %, reported as 360 %, and 38.9/12 × 100 = 324.2 %, reported as 325 %. Mean of the unrounded values = 341.1 %, reported as 340 %.
-
Failure mode: cohesive in all three specimens.
ISO 11600 classes a sealant as HM if its secant modulus exceeds 0.4 N/mm² at +23 °C or 0.6 N/mm² at −20 °C, using the mean of three measurements rounded to one decimal place. Here the means round to 0.4 and 0.5 N/mm². Neither exceeds its limit, so the modulus results fall in the LM range. A full ISO 11600 classification also needs the other required tests, such as ISO 8340 maintained extension, ISO 7389 elastic recovery and the adhesion/cohesion tests. Note how close the 23 °C mean sits to the limit: a few newtons of extra force from a misaligned holder would change it.
Typical results and what to report
Low-modulus façade sealants sit at or below 0.4 N/mm² at 100 % and 23 °C. High-modulus and glazing products are higher. All sealants stiffen at −20 °C, so the cold modulus is always the higher of the two. Elastic sealants usually stretch well beyond 100 % before breaking, while plastic sealants (ISO 11600 classes 12.5P and 7.5P) break at much lower elongations. Cohesive failure is the expected result for a well-bonded sealant. Repeated adhesive failure on one substrate points to a primer, cleaning or compatibility problem, not a sealant property.
The ISO 8339:2005 test report includes:
-
Name of the laboratory, date of test and a reference to ISO 8339.
-
Sealant name, chemical type, colour and batch.
-
Substrate used, primer (if any) and conditioning method (A or B).
-
Secant modulus of each specimen at the chosen elongation (100 %, 60 % or as agreed) and the mean of the three.
-
Elongation at break of each specimen and the mean.
-
Type of break, adhesive and/or cohesive, for each specimen.
-
Any deviation from the standard, for example non-standard substrate size or test temperature.
Common ISO 8339 errors
-
Leaving the spacers in. The force curve rises steeply from zero and the modulus is meaningless.
-
Bending the joint. Rigid connections or holders that grip only one end of the substrate peel the bead from one end and lower the elongation at break. Self-aligning swivels and full-width bearing prevent this.
-
Wrong speed. A frame that cannot run below 13 mm/min is outside the 5.5 ± 0.7 mm/min tolerance. Faster rates raise the modulus of most sealants.
-
Warm cold tests. Taking specimens out of a freezer and testing them on an open bench breaks the −20 ± 2 °C requirement within minutes. Extend them inside a chamber.
-
Short cure. Testing before 28 days, or at low humidity for moisture-curing products, under-cures the bead and lowers the modulus.
-
Air voids and poor wetting. These cause early cohesive or adhesive breaks and scatter in elongation at break.
-
Rounding too early. Calculate each specimen to 0.01 N/mm². Round the mean to one decimal only when classifying to ISO 11600.
-
Confusing ISO 8339 with ISO 8340. ISO 8340 holds the specimen at a fixed extension and checks for failure. It does not measure elongation at break.
ISO 8339 vs ASTM, EN and related ISO standards
EN ISO 8339 is the European adoption of the same method and is cited in sealant product standards such as the EN 15651 series. The results are interchangeable when the same edition is used. In North America, sealant tensile adhesion is often tested to ASTM C1135, which also uses an H-shaped specimen. Its specimen dimensions and test rate are inch-based and different from ISO 8339, so do not mix data sets or compare moduli directly. If you test cured sealant as free-film dumbbells rather than joints, that is a rubber-style tensile test. See our ISO 37 and ASTM D412 guides.
Related ISO sealant standards:
-
ISO 8340: tensile properties at maintained extension. The specimen is held stretched (for example at 60 % or 100 %) for 24 h and inspected for failure. It uses the same H-block, so the same fixture serves both tests.
-
ISO 11600: classification and requirements for building sealants, types F and G, classes 25, 20, 12.5 and 7.5 with LM/HM and E/P subclasses. It draws on ISO 8339, ISO 8340 and the other methods listed here.
-
ISO 9046: adhesion/cohesion properties at constant temperature, with cyclic extension and compression.
-
ISO 9047: adhesion/cohesion properties at variable temperatures.
-
ISO 7389: elastic recovery, which separates elastic (E) from plastic (P) class 12.5 sealants.
-
ISO 10590: tensile properties at maintained extension after immersion in water.
-
ISO 13640: specifications for the mortar, glass and aluminium test substrates.
-
ISO 6927: sealant vocabulary.
For other standards we cover, see our ISO standards hub and ASTM standards hub.
ISO 8339 equipment summary
-
Fixture: Universal Grip ISO 8339 H-block tensile fixture (UGC-ISO8339-TF), 1 kN standard. See tensile grips and adapters.
-
QC frame at 23 °C: Mark-10 F305 or F505 with the low-speed option for 5.5 mm/min.
-
Full program including −20 °C: Galdabini 2.5 kN or 5 kN benchtop UTM with an environmental chamber.
-
Optional measurement: video extensometer for direct gap measurement, especially inside a chamber.
-
Software: test software to calculate secant modulus at 60 % or 100 % and elongation at break automatically.
-
Application background: tensile testing and adhesives testing.
ISO 8339 FAQ
What is ISO 8339?
ISO 8339 is the ISO test method for the tensile properties of building construction sealants. A 12 × 12 × 50 mm sealant bead cured between two substrates (an H-block) is extended at 5.5 mm/min to break, giving secant tensile modulus, elongation at break and failure mode.
What is the current edition of ISO 8339?
ISO 8339:2005, the second edition, was confirmed by ISO in 2020. A third edition, ISO/DIS 8339, is in development under the title Building and civil engineering sealants. Check whether it has been published before updating your procedures.
What are the ISO 8339 specimen dimensions?
The sealant bead is 12 mm wide, 12 mm deep and 50 mm long, bonded between two substrates of the same material. The bonded area used in the modulus calculation is 12 × 50 = 600 mm². Other substrate sizes are allowed if the bead and bonded area match.
What test speed does ISO 8339 use?
The specimen is extended at 5.5 ± 0.7 mm/min until it ruptures. Many compact test stands cannot run that slowly without a low-speed option, so check the speed range of your frame.
How many specimens are required?
Three specimens for each substrate type and each test temperature. Testing one substrate at 23 °C and −20 °C needs six specimens.
What is the difference between Method A and Method B conditioning?
Method A is 28 days at 23 °C and 50 % RH. Method B adds three cycles of 70 °C oven exposure and distilled water immersion after Method A, followed by 24 h at standard conditions. The standard notes that Method B does not indicate durability.
How is secant modulus calculated in ISO 8339?
Divide the force at the chosen elongation, usually 100 % or 60 %, by the initial cross-section of 600 mm². For example, 240 N at 100 % elongation gives 0.40 N/mm². Report each specimen to 0.01 N/mm².
What makes a sealant low modulus or high modulus?
Under ISO 11600, a class 25 or 20 sealant is high modulus (HM) if its secant modulus exceeds 0.4 N/mm² at +23 °C or 0.6 N/mm² at −20 °C, based on the mean of three results rounded to one decimal. Otherwise it is low modulus (LM).
What is the difference between ISO 8339 and ISO 8340?
ISO 8339 extends the H-block to break and measures modulus and elongation at break. ISO 8340 holds the specimen at a fixed extension for 24 h and checks for failure. Both use the same specimen and the same holders.
Can a Mark-10 tester run ISO 8339?
Yes, for 23 °C testing, if it has the low-speed option, because the standard speed range starts at 13 mm/min. The F305 or F505 suits most sealants. For −20 °C testing inside a chamber, a Galdabini benchtop UTM with an environmental chamber is the better choice.
Is there an ASTM equivalent to ISO 8339?
There is no identical ASTM method. ASTM C1135 uses a similar H-shaped specimen for sealant tensile adhesion, but with different dimensions and test rate, so results are not directly comparable. EN ISO 8339 is identical to ISO 8339.