ISO 15754
Z-Directional Tensile Strength of Paper and Board

ISO 15754 Z-Directional Tensile Fixture for Paper and Board by Universal Grip

Downloads: ISO 15754 Z-Directional Tensile Fixture for Paper and Board – Universal Grip Data Sheet (PDF)

Written by Chris Thomas, Universal Grip Company · Reviewed by Frank Bertini · Updated October 27, 2026

ISO 15754 is the international method for determining the z-directional tensile strength (ZDT) of paper and board: the stress needed to pull a sheet apart perpendicular to its plane. A test piece is bonded with double-sided adhesive tape between two platens, pressed together, then pulled apart until it splits internally. The maximum force divided by the test area gives the result in kPa, a direct measure of the internal (fiber-to-fiber and ply-to-ply) bond.

Board mills, converters and printers use ZDT to control refining, starch and ply bonding, and to prevent delamination in printing, creasing and gluing. Universal Grip makes an ISO 15754 z-directional tensile fixture with guided, parallel platens and a five-position sliding lower platen, described in the equipment section below.

In this guide: What ISO 15754 Measures · Current Edition and Scope of ISO 15754 · Test Pieces, Sampling and Conditioning · Apparatus: Platens, Tape, Machine and Load Cell · ISO 15754 Test Procedure Step by Step · Calculating Z-Directional Tensile Strength · Valid and Invalid Breaks: Interpreting Results · What Influences ZDT: Material and Test Factors · What to Include in the ISO 15754 Test Report · Common ISO 15754 Errors · ISO 15754 vs TAPPI T541 · Related Paper and Board Strength Tests · ISO 15754 Equipment from Universal Grip · FAQ

What ISO 15754 Measures

Paper and board are strong in-plane but weak through the thickness, because the z-direction is held together only by fiber-to-fiber bonds and, in multi-ply board, by the bond between plies. ISO 15754 loads that weak direction directly: the force acts normal to the sheet, so the test piece fails at its weakest layer or interface.

The result, z-directional tensile strength, is commonly called ZDT, internal bond strength or z-strength. It is used to:

  • Control refining, wet-pressing and starch or additive dosage that drive internal bonding.

  • Check ply bonding in multi-ply folding boxboard, liquid packaging board and linerboard.

  • Predict resistance to splitting, blistering and picking under high-tack printing inks.

  • Diagnose delamination at creases, folds and glue flaps in converting.

Note: ZDT is a quasi-static tensile test. It is different from the Scott-type internal bond test, which measures the energy absorbed when a pendulum delaminates the sheet at high speed. The two results do not correlate reliably, so do not substitute one for the other in a specification.

Current Edition and Scope of ISO 15754

The current version is ISO 15754:2009, the first edition, published in March 2009 by ISO/TC 6/SC 2 (Test methods and quality specifications for paper and board). ISO reviewed and confirmed it in 2025, so the 2009 edition remains current. It is adopted nationally, for example as BS ISO 15754:2009 and DIN ISO 15754:2010-04.

Key points from the scope:

  • It applies to paper and board.

  • It does not apply to corrugated fibreboard. Corrugated board is a structure of liners and fluting, and its out-of-plane behavior is tested with other methods such as flat crush (ISO 3035).

  • For papers below about 60 g/m², results should be treated with caution, because the tape can penetrate or reinforce a thin sheet. The standard notes that the lower grammage limit cannot be stated exactly.

  • The method does not give an absolute material strength: the tape, the pressing conditions and the test speed all influence the result. ZDT values are therefore comparable only when these are held constant.

Test Pieces, Sampling and Conditioning

Test pieces are cut from the sample so that each fully covers the platen test area with margin, free from folds, wrinkles, creases or other visible defects. Handle them by the edges only: fingerprints and skin oils on the faces interfere with tape adhesion.

  • Sampling: take samples in accordance with ISO 186 so that results represent the lot.

  • Conditioning: condition and test in the standard atmosphere of ISO 187, 23 °C ± 1 °C and 50% ± 2% relative humidity. Moisture strongly affects fiber bonding, so ZDT is very sensitive to conditioning.

  • Test area: the result is calculated on the platen area, so the platen area must be known accurately. Many instruments use a 1 in² (645 mm²) square platen, the same area specified in TAPPI T541.

  • Number of tests: follow the number specified in the standard; using several test pieces per sample is necessary because ZDT has more scatter than in-plane tensile tests.

  • Sides: mark the top and wire sides (or the print side) consistently, since layered sheets can behave differently depending on orientation.

Note: Where this page gives TAPPI T541 values (for example, 50 mm × 50 mm minimum test pieces and five specimens per sample), they come from the TAPPI method. Check the ISO 15754 text for the ISO-specific values before writing a test procedure.

Apparatus: Platens, Tape, Machine and Load Cell

Platens and alignment

The apparatus is two flat platens: one fixed and one attached to the moving crosshead through the load cell. The platens must stay parallel during both the compression step and the pull. Out-of-parallel platens press the tape unevenly and then peel the test piece from one edge instead of loading it in uniform tension, which lowers the result and increases scatter. High transverse stiffness also matters, so the platens do not shift sideways as the test piece splits.

Double-sided tape

The test piece is attached to each platen with double-sided pressure-sensitive tape. The tape is part of the measuring system: its adhesion to the platen and to the paper must be higher than the internal strength of the test piece, and its adhesive must not soak far into the sheet. Use one tape type consistently, record it in the report, and requalify when changing tape brand or lot.

Machine and load cell

Any constant-rate universal testing machine that can apply a controlled compressive force, hold it for a set dwell, then reverse into tension at a constant rate can run ISO 15754. A benchtop frame is typical. Forces are modest: on a 645 mm² platen, 1,000 kPa of z-strength is 645 N. Size the load cell so both the compression force and the expected peak tensile forces fall within its accurate range.

ISO 15754 Test Procedure Step by Step

  • 1. Condition the test pieces in the ISO 187 atmosphere and run the test in the same atmosphere.

  • 2. Clean the platens of old tape residue and fiber. Residue changes the effective area and tape adhesion.

  • 3. Apply double-sided tape to the platen faces (or to both faces of the test piece), avoiding air bubbles and creases in the tape.

  • 4. Place the test piece on the lower platen, centred within the test area, with the marked side oriented consistently.

  • 5. Bring the upper platen down and press the assembly at the specified compressive force for the specified dwell time. This step wets the tape into both surfaces and must be identical for every test.

  • 6. Reverse the crosshead and pull the platens apart at the specified rate until the test piece splits. Record the maximum force.

  • 7. Inspect both platens. Accept the test only if the split is within the paper or board; reject it if the tape released from the platen or from the paper.

  • 8. Remove the split halves and tape, then repeat for the remaining test pieces.

Pressing force, dwell and separation rate are fixed by the standard because each affects the answer: a higher pressing force or longer dwell can densify the sheet and drive adhesive deeper into it, and a faster pull gives a higher peak. Program them into the testing software as a fixed method so operators cannot change them between tests.

Calculating Z-Directional Tensile Strength

The z-directional tensile strength is the maximum tensile force divided by the test area:

  • σZD = F / A

  • F: maximum force, in N.

  • A: platen (test) area, in mm².

  • Result: F/A in N/mm² equals MPa; multiply by 1,000 to report in kPa, the usual unit for ZDT.

For a 1 in² platen (645.16 mm²), 1 N corresponds to 1.55 kPa, which is why TAPPI T541 converts a force reading in newtons to kPa by multiplying by 1.55.

Worked example

Five test pieces of a folding boxboard are tested on a 645.16 mm² platen. Maximum forces are 402 N, 388 N, 415 N, 371 N and 396 N, and all five split within the board.

  • 402 N ÷ 645.16 mm² = 0.623 N/mm² = 623 kPa

  • 388 N ÷ 645.16 mm² = 601 kPa

  • 415 N ÷ 645.16 mm² = 643 kPa

  • 371 N ÷ 645.16 mm² = 575 kPa

  • 396 N ÷ 645.16 mm² = 614 kPa

  • Mean: 611 kPa; standard deviation: 25 kPa; coefficient of variation: 4.2%.

Check: the mean force is 394.4 N, and 394.4 × 1.55 = 611 kPa, which matches the mean of the individual results. Report the mean and the variation (standard deviation or coefficient of variation) together with the number of valid tests.

Valid and Invalid Breaks: Interpreting Results

A valid ZDT test fails inside the paper or board. Looking at the split surfaces tells you as much as the number:

  • Fibers on both tapes across the whole area: a valid split within the sheet. The value reflects the internal bond.

  • Split along a ply line in multi-ply board: valid, and it shows that the ply bond is the weak link. Starch spray or ply-bonding additives are the usual levers.

  • Split just under a coating layer: valid for the product, but it indicates coating-base adhesion or surface sizing is weaker than the base sheet.

  • Bare tape or clean platen: invalid. The tape released from the paper or the platen. Discard the result and check tape type, cleanliness and pressing step.

  • Split confined to one corner or edge: suspect platen misalignment or an off-centre test piece.

Because the tape can reinforce the surface layers, a very high result on thin, porous or low-grammage paper may describe the tape-paper composite more than the paper. That is the reason for the 60 g/m² caution in the standard.

What Influences ZDT: Material and Test Factors

ZDT is one of the most process-sensitive board properties, which is why mills track it closely. The main material factors are:

  • Refining: more refining increases fiber flexibility and bonded area, and ZDT normally rises with it.

  • Wet pressing and density: higher pressing consolidates the sheet and increases bonding through the thickness, at the cost of bulk and bending stiffness.

  • Starch and bonding additives: surface or spray starch and dry-strength additives raise ZDT, especially at ply interfaces in multi-ply board.

  • Fillers and fines: high filler loadings sit between fibers and reduce bonding.

  • Furnish and layering: recycled fiber, mechanical pulp middle plies and the strength of each ply interface decide where the board splits.

  • Moisture content: wetter sheets have weaker fiber bonds, so conditioning controls a large part of the variation.

Test factors matter almost as much: the tape, the compressive force and dwell, the separation rate, platen parallelism and cleanliness. Because the standard itself states that these influence the result, hold them constant and treat ZDT as a comparative value within one method and one laboratory setup. When a mill and a converter disagree on ZDT, compare the test conditions before debating the board.

What to Include in the ISO 15754 Test Report

A complete report allows another laboratory to reproduce the conditions that influence ZDT. Include at least:

  • A reference to ISO 15754:2009.

  • Identification of the sample, including grade and grammage, and the side orientation tested.

  • Conditioning and test atmosphere.

  • Platen (test) area.

  • Tape type and identification.

  • Number of valid tests and the number rejected for tape failure.

  • Mean z-directional tensile strength in kPa and its variation (standard deviation or coefficient of variation).

  • Any deviation from the standard procedure.

Common ISO 15754 Errors

  • Mixing methods: running TAPPI T541 settings and reporting the result as ISO 15754 (or the reverse). The press and pull conditions influence the value, so name the method you actually followed.

  • Changing tape without checking: a new tape lot or brand can shift results. Requalify with a reference board.

  • Dirty platens: residue from previous tests reduces tape adhesion and changes the effective area.

  • Poor parallelism: unguided or worn platens peel the test piece from one edge.

  • Uncontrolled atmosphere: testing outside 23 °C and 50% RH, or before the sheet has reached moisture equilibrium.

  • Testing corrugated board: ISO 15754 excludes corrugated fibreboard.

  • Averaging invalid tests: results with tape failure must be discarded, not averaged.

ISO 15754 vs TAPPI T541

There is no ASTM equivalent to ISO 15754. The North American counterpart is TAPPI T541, "Internal bond strength of paperboard (z-direction tensile)", current as ANSI/TAPPI T 541 om-21. Both use double-sided tape, a compression step and a perpendicular pull, and both report in kPa, but they are separate methods. Key T541 parameters are:

  • Platen area: 6.45 cm² (1 in²), with one self-aligning platen.

  • Test pieces: at least 50 mm × 50 mm (2 in × 2 in); five per sample.

  • Tape: double-sided pressure-sensitive tape, 50 mm (2 in) wide; tape identity is reported.

  • Compression: 890 N ± 13.5 N (200 lbf) contact force, held for 6 s ± 1 s.

  • Tension rate: 66 mm/min ± 5 mm/min (2.6 in/min).

  • Conditioning: TAPPI T402 (23 °C, 50% RH).

  • Calculation: force in N × 1.55 = kPa.

  • Precision: TAPPI interlaboratory data report repeatability around 6% and reproducibility around 34%.

The large reproducibility figure shows how strongly ZDT depends on the apparatus, tape and technique of each laboratory. When comparing a supplier certificate with in-house data, confirm which standard, tape and settings were used before treating a difference as real. A closely related Nordic method, SCAN-P 80, is also cited by some instrument makers.

Related Paper and Board Strength Tests

  • Scott-type internal bond: ISO 16260 (2025 edition) and TAPPI T569 measure the energy to delaminate a sheet with a pendulum, a high-rate test that does not correlate directly with ZDT.

  • In-plane tensile strength: ISO 1924-2 (constant rate of elongation, 20 mm/min) and ASTM D828.

  • Corrugated board: flat crush resistance by ISO 3035, since ISO 15754 excludes corrugated fibreboard.

  • Ply bond by peeling: peel-type ply bond methods load the interface as a peel rather than in uniform tension and give a different number from ZDT.

A complete board characterization often combines ZDT (internal bond), Scott bond (impact delamination) and in-plane tensile strength, because each responds differently to refining, pressing and starch.

ISO 15754 Equipment from Universal Grip

ISO 15754 Z-Directional Tensile Fixture (part ref. UGC-ISO15754-TG)

Our die-set style fixture runs the full ISO 15754 sequence. Test pieces are bonded with double-sided tape between upper and lower platens, pressed together under guided alignment, then pulled apart perpendicular to the sheet plane. A sliding multi-position lower platen tests several test pieces in sequence.

  • Test method: z-directional tensile strength per ISO 15754.

  • Loading: compression, then tension normal to the sheet plane, in the same fixture.

  • Alignment: guide posts and bushings keep the upper and lower platens parallel.

  • Throughput: a multi-position lower platen on a linear slide tests five test pieces in sequence, with indexed positions for repeatable placement.

  • Contact surfaces: flat platens with numbered test piece positions.

  • Specimens: paper or board squares bonded with double-sided tape.

  • Load capacity: 5 kN standard; higher capacities on request.

  • Materials: anodized aluminium and stainless steel.

  • Machine connection: pin adapter with locking collar, or threaded adapter; supplied with adapters to suit your load frame.

  • Compatible frames: electromechanical and servo-hydraulic universal test machines.

When ordering, specify the test piece size, number of positions, tape type, required capacity and machine connection. Typical applications are paperboard and folding boxboard, linerboard and multi-ply board, coated papers and laminates, and mill quality control.

For other connection styles see our adapters, and for the full range of standards we support see our ISO test standards index. Send us your platen size and frame model and contact us for a quote.

ISO 15754 FAQ

What is ISO 15754?

ISO 15754 is the ISO method for determining the z-directional tensile strength (ZDT) of paper and board. A test piece is bonded with double-sided tape between two platens, pressed, then pulled apart perpendicular to the sheet plane. The maximum force divided by the test area gives the result in kPa.

What is the current edition of ISO 15754?

The current version is ISO 15754:2009, the first edition. ISO reviewed and confirmed it in 2025, so it remains current.

What does z-directional tensile strength tell you?

It measures the internal bond of the sheet: how well fibers and plies hold together through the thickness. Low ZDT predicts splitting, blistering and delamination in printing, creasing and gluing.

Can ISO 15754 be used for corrugated board?

No. The scope of ISO 15754 excludes corrugated fibreboard. Corrugated board is usually evaluated with other methods such as flat crush resistance to ISO 3035.

Is ISO 15754 suitable for thin papers?

Use caution below about 60 g/m². The double-sided tape can reinforce a thin sheet, so the result may reflect the tape-paper composite rather than the paper alone, and the standard notes that the lower grammage limit cannot be stated exactly.

How is ZDT calculated?

Divide the maximum force by the test area: σZD = F / A. For example, 402 N on a 645.16 mm² (1 in²) platen gives 0.623 N/mm², or 623 kPa. On a 1 in² platen, every newton equals 1.55 kPa.

What is the difference between ISO 15754 and TAPPI T541?

Both are z-direction tensile tests with tape, a compression step and a perpendicular pull, reporting in kPa. TAPPI T541 specifies a 1 in² platen, 890 N compression for 6 s ± 1 s and a 66 mm/min ± 5 mm/min pull on five test pieces; ISO 15754 sets its own conditions, so results should be labeled with the method actually used.

Is there an ASTM equivalent to ISO 15754?

There is no ASTM equivalent. The North American counterpart is TAPPI T541, "Internal bond strength of paperboard (z-direction tensile)".

What is the difference between ZDT and Scott bond?

ZDT is a slow tensile test that reports a stress in kPa. Scott-type internal bond (ISO 16260, TAPPI T569) uses a pendulum to delaminate the sheet at high speed and reports energy. The two do not correlate directly, so they are not interchangeable.

When is an ISO 15754 result invalid?

A result is invalid if the tape separates from the platen or from the paper instead of the sheet splitting internally. Discard those tests, clean the platens, and check the tape and pressing step before continuing.

What fixture do I need for ISO 15754?

You need two flat, parallel platens that can press the taped test piece and then pull it apart without tilting. Universal Grip's ISO 15754 fixture uses guide posts and bushings for parallelism and a five-position sliding lower platen, 5 kN standard. Contact us for a quote.

Need a fixture, grips or a complete test system for ISO 15754? Contact Universal Grip with your material, specimen size and machine connection and we will quote the right setup.