ISO 13314
Compression Test for Porous and Cellular Metals

Downloads: ISO 13314 Compression Platens for Porous and Cellular Metals – Universal Grip Data Sheet (PDF)
Written by Chris Thomas, Universal Grip Company · Reviewed by Frank Bertini · Updated October 31, 2026
ISO 13314 is the international test method for the quasi-static compression of porous and cellular metals with a porosity of 50 % or more: aluminium and other metal foams, metal sponges, sintered porous metals and, increasingly, additively manufactured lattice structures. Dense-metal compression methods do not work for these materials, because a foam does not yield and then barrel. It shows a short quasi-elastic rise, a long, nearly flat plateau while cells buckle and collapse, and then a steep climb as the cells are crushed shut. ISO 13314 defines how to size the specimen against the pore size, how fast to compress it and how to pull plateau stress, plateau end, energy absorption and proof strengths out of the stress-strain curve. Crash-absorber developers, implant and filter makers, lattice designers and university labs all use it. It is easy to get wrong: specimens that are too small for the pore size give scattered results, crosshead compliance distorts the early strain, and platens that are not hard, flat and parallel spoil the plateau. This guide covers the current edition, specimens, speed, the machine and compression platens you need, a worked calculation, typical results, common errors and related standards.
ISO 13314 at a glance
-
Current edition: ISO 13314:2011, first edition, prepared by ISO/TC 164/SC 2 (ductility testing). ISO lists it as reviewed and confirmed in 2022, so the 2011 text remains current.
-
Full title: Mechanical testing of metals — Ductility testing — Compression test for porous and cellular metals.
-
Scope: compressive properties of porous and cellular metals with porosity of 50 % or more, at ambient temperature and quasi-static strain rates.
-
Specimen: cylindrical (recommended) or rectangular; every dimension at least 10 times the average pore size and at least 10 mm; height-to-diameter or height-to-edge ratio between 1 and 2.
-
Number of specimens: at least three, five recommended, plus a preliminary specimen when an estimate of plateau stress is needed.
-
Test speed: constant crosshead speed giving an initial strain rate between 10⁻³ s⁻¹ and 10⁻² s⁻¹.
-
Temperature: ambient, 10 °C to 35 °C, or 23 ± 5 °C where tight control is required.
-
Platens: plane-ground, mirror-finished, minimum 60 HRC.
-
Results: plateau stress, first maximum compressive strength, plateau end, energy absorption and energy absorption efficiency; optionally quasi-elastic gradient, elastic gradient, compressive offset stress and compressive proof strength.
-
Related standards: ISO 17340 (high-speed compression of porous metals), ISO 7500-1 (force verification), ISO 9513 (extensometer calibration).
What ISO 13314 measures and who uses it
The whole point of a metal foam is to absorb energy at a controlled, nearly constant stress. ISO 13314 turns the compressive stress-strain curve into a few numbers designers can compare across materials and suppliers.
-
Plateau stress: the arithmetic mean of the stresses at strain intervals of 0.1 % or smaller between 20 % and 30 %, or 20 % and 40 %, compressive strain. The range used depends on where the plateau ends and must be reported.
-
First maximum compressive strength: the stress at the first local maximum of the curve, if there is one. Many closed-cell foams show a peak followed by a drop; many open-cell materials do not, in which case it cannot be determined.
-
Plateau end: the point where the stress reaches 1.3 times the plateau stress, marking the onset of densification.
-
Energy absorption W: the area under the stress-strain curve up to 50 % strain or up to the plateau end strain, in MJ/m³.
-
Energy absorption efficiency: energy absorption divided by the product of the maximum compressive stress within the strain range and the size of that strain range, as a percentage. An ideal absorber with a perfectly flat curve approaches 100 %.
-
Optional values: quasi-elastic gradient (slope of the linear loading region), elastic gradient (slope from an unloading-reloading loop between 70 % and 20 % of plateau stress), compressive offset stress (at 0.2 % plastic strain) and compressive proof strength (at 1.0 % plastic strain unless otherwise specified).
Users include automotive and rail crash-energy absorber developers, aerospace sandwich-core designers, makers of porous implants, filters and heat-exchanger media, and teams qualifying additively manufactured lattice structures, where ISO 13314 is a common reference even though lattices are not foams in the traditional sense.
Test specimens
Shape and size
-
Shape: cylindrical specimens are recommended; square or rectangular cross-sections are allowed.
-
Size against pore size: all spatial dimensions (diameter D0 or edge W0, and height) must be at least 10 times the average pore size, and not less than 10 mm. A foam with 4 mm average pores therefore needs at least a 40 mm diameter or edge.
-
Aspect ratio: height to diameter (H0:D0) or height to edge (H0:W0) between 1 and 2.
-
Record: specimen geometry, average pore size and whether the porosity is open or closed.
Number and sampling
-
Number: at least three specimens; five or more are recommended because cellular metals scatter far more than dense metals.
-
Preliminary specimen: one extra specimen is used for a preliminary test that gives an initial estimate of the plateau stress, needed to set the unloading points if you determine the elastic gradient.
-
Cutting: the cutting method must not change the material properties. Wire EDM, fine band sawing and careful milling are common choices; abrasive or blunt cutting can smear or crush the surface cells and soften the start of the curve.
-
Faces: loading faces should be flat and parallel so the platens contact the whole cross-section at the start of the test.
Measurement
Measure width, thickness or diameter and height to 0.1 mm, preferably at three or more points, and calculate the initial cross-sectional area A0. Record density and porosity in the report; ISO 13314 lists material, density, porosity, pore type and average pore size among the required items.
Conditioning and test temperature
ISO 13314 does not require a conditioning period. Tests are run at ambient temperature between 10 °C and 35 °C, and the temperature is recorded if relevant. Where tight control is needed, test at 23 ± 5 °C. For materials that oxidise or absorb moisture in their pores, such as some sintered metals, store specimens dry and note any storage conditions. An environmental chamber is only needed if you deliberately test outside the standard's temperature range for research.
Test speed and machine requirements
-
Machine: a compression testing machine verified to ISO 7500-1 that can run at constant crosshead speed.
-
Speed: choose a constant crosshead speed giving an initial strain rate between 10⁻³ s⁻¹ and 10⁻² s⁻¹. Crosshead speed = strain rate × H0. For a 40 mm tall specimen that is 0.04 to 0.4 mm/s, or 2.4 to 24 mm/min. Record the crosshead speed or the initial strain rate.
-
Data rate: record force and displacement at 30 Hz or faster up to 5 % strain (or the proof-strength strain if larger), then at 10 Hz or faster.
-
Strain measurement: an extensometer of at least class 1 to ISO 9513, or strain calculated from measured displacement.
-
Stroke: compression to 50 % strain or the plateau end means a stroke of at least half the specimen height, and often more.
The Universal Grip ISO 13314 compression platens
Our ISO 13314 compression platen set (part ref. UGC-ISO13314-CP) is a hardened platen set for testing metal foams and other porous or cellular metals. Large ground platens with concentric centring rings support the specimen, and adjustable side stops on the platen flange help centre it before it is compressed through its plateau and densification regions.
-
Large-diameter platens, hardened tool steel to about 60 HRC.
-
Concentric centring rings engraved on both platen faces, so cylinders and cubes go on the load axis every time.
-
Adjustable side stops with knobs that centre the specimen before the test.
-
Ground, parallel faces for uniform load distribution across a specimen whose cells must all see the same strain.
-
Load capacity: 100 kN standard; higher capacities on request.
-
Specimens: cubic or cylindrical porous metal specimens.
-
Machine connection: clevis pin or threaded adapter to suit your frame; compatible with electromechanical and servo-hydraulic universal test machines.
ISO 13314 asks for plane-ground, mirror-finished platens with a minimum hardness of 60 HRC. When you order, give us the specimen size, the platen diameter, the capacity you need, your machine connection and the face finish and hardness your procedure specifies, and we will confirm the configuration in the quote. Platen diameter should comfortably exceed the specimen's largest dimension, because foam specimens spread very little but lattices can buckle sideways. See all compression platens and compression fixtures, and our compression testing application page.
Choosing a testing machine
Force depends on plateau stress and specimen area, and the area is driven by pore size. Low-density aluminium foams can have plateau stresses of only a few MPa, while dense foams and metal lattices can reach tens of MPa. Remember that force climbs steeply past the plateau end, so if you run into densification, size the machine for that, not the plateau.
-
Example: fine-pore foam: 30 mm diameter cylinder (A0 ≈ 707 mm²) at 5 MPa plateau stress needs about 3.5 kN on the plateau, and about 4.6 kN at the plateau end (1.3 times).
-
Example: coarse-pore foam: 5 mm pores need a 50 mm specimen. A 50 mm cube (2,500 mm²) at 10 MPa needs 25 kN on the plateau.
-
Example: titanium lattice: a 40 mm cylinder (about 1,257 mm²) at 60 MPa needs about 75 kN before densification.
Mark-10 force testers can handle small, low-strength foam specimens for screening or incoming QC. The Mark-10 F1505 (1,500 lbF, about 6.7 kN, 813 mm travel, 10 to 600 mm/min) covers the fine-pore example on the plateau, and the F505 (about 2.2 kN) suits very light foams. The low-speed option on the F105 to F505 (down to 0.5 mm/min) reaches the 10⁻³ s⁻¹ end of the range. For anything stronger, larger, or run into densification, and for formal ISO 13314 reporting, use a universal testing machine and check that your force calibration meets ISO 7500-1.
-
Galdabini 10 to 50 kN benchtop UTMs: the 10 kN, 25 kN and 50 kN frames cover most aluminium foams.
-
Galdabini 100 kN benchtop: the 100 kN UTM matches the 100 kN rating of our platens and handles dense foams and most lattices.
-
Floor-standing frames: a 200 kN or 250 kN UTM, with higher-capacity platens, for large specimens, high-strength lattices or tests taken deep into densification.
Extensometers and strain measurement
ISO 13314 lets you take strain from an extensometer (class 1 to ISO 9513) or calculate it from displacement. In practice, clip-on extensometers on the specimen itself are a poor choice: cells collapse under the knife edges and the specimen surface crushes. Most labs use crosshead displacement with a machine compliance correction, which matters most for the quasi-elastic gradient and proof strengths at small strains. A video extensometer tracking marks on the two platens gives a non-contact, compliance-free platen-to-platen displacement and survives the full crush; see our extensometers page for other options. If you only report plateau stress, plateau end and energy absorption, corrected crosshead displacement is usually sufficient.
ISO 13314 test procedure step by step
-
1. Characterise the material. Record density, porosity, open or closed pores and average pore size.
-
2. Size and cut specimens. Make every dimension at least 10 times the average pore size and at least 10 mm, with H0:D0 or H0:W0 between 1 and 2, using a cutting method that does not damage cells.
-
3. Measure. Diameter or width and thickness, and height, to 0.1 mm at three or more points; calculate A0.
-
4. Set up. Fit the platens, check parallelism, zero the force and set crosshead speed = target strain rate × H0.
-
5. Preliminary test (if needed). Compress one specimen to estimate the plateau stress, used to set the unloading points.
-
6. Centre the specimen. Use the centring rings and side stops so it sits on the load axis, then retract the side stops so they do not touch the specimen.
-
7. Compress. Run at constant crosshead speed and record the force-displacement curve at the required data rate. For the optional elastic gradient, unload from 70 % to 20 % of the estimated plateau stress and reload.
-
8. Continue to at least the plateau end or 50 % strain, whichever is required for energy absorption. If the plateau end is unclear, choose another stress on the curve and record that choice.
-
9. Set zero strain where the quasi-elastic or elastic gradient line crosses the strain axis, then calculate results.
-
10. Repeat for at least three, preferably five, specimens and report.
Calculations with a worked example
-
Specimen: closed-cell aluminium foam cylinder, D0 = 30.0 mm, H0 = 45.0 mm, average pore size 2.5 mm. Check: 10 × 2.5 = 25 mm ≤ 30 mm, and H0:D0 = 1.5, within 1 to 2.
-
Area: A0 = π × 15.0² = 706.9 mm².
-
Speed: for an initial strain rate of 5 × 10⁻³ s⁻¹, crosshead speed = 0.005 × 45.0 = 0.225 mm/s = 13.5 mm/min.
-
Strain: compressive strain = displacement / H0. At 9.0 mm, strain = 9.0 / 45.0 = 20 %; at 13.5 mm, 30 %; at 22.5 mm, 50 %.
-
Plateau stress: the mean force between 20 % and 30 % strain is 3,180 N, so σpl = 3,180 / 706.9 = 4.50 MPa.
-
Plateau end: 1.3 × 4.50 = 5.85 MPa, a force of 5.85 × 706.9 ≈ 4,135 N. The curve reaches this at 52 % strain, so the plateau end strain is 52 %.
-
Energy absorption: numerical integration of the stress-strain curve from zero to 50 % strain gives W = 2.19 MJ/m³ (1 MPa × 1 strain = 1 MJ/m³). Specimen volume = 706.9 × 45.0 ≈ 31,810 mm³ = 3.181 × 10⁻⁵ m³, so the absorbed energy is 2.19 × 10⁶ × 3.181 × 10⁻⁵ ≈ 69.7 J.
-
Efficiency: the maximum stress up to 50 % strain is 5.20 MPa, so efficiency = 2.19 / (5.20 × 0.50) × 100 = 2.19 / 2.60 × 100 ≈ 84 %.
Typical results and what to report
Results depend strongly on density and cell structure. Closed-cell aluminium foams often show a first maximum followed by a slightly serrated plateau; open-cell foams and many lattices rise more smoothly; brittle lattices may show sharp drops as layers fail. Expect a coefficient of variation in plateau stress far higher than for dense metals, which is why five specimens are recommended. ISO 13314 requires the report to include:
-
Reference to ISO 13314:2011, and product name and designation.
-
Material, density, porosity, pore type (open or closed) and average pore size.
-
Specimen dimensions and H0:D0 or H0:W0 ratio, and number of specimens.
-
Test conditions, including temperature and lubrication if used, and the compression speed or strain rate.
-
Plateau stress with its strain range, first maximum compressive strength if present, plateau end strain and how it was determined, energy absorption with its upper strain limit, energy absorption efficiency, and the stress-strain diagrams.
-
Optionally: machine type and range, sample preparation, quasi-elastic gradient, compressive offset stress, elastic gradient, compressive proof strength and statistics.
Common errors in ISO 13314 testing
-
Specimens too small for the pore size, so a handful of cells controls the result.
-
Damaged surface cells from sawing or grinding, which soften the start of the curve and lower the first maximum.
-
Non-parallel faces or platens, which crush one edge first and tilt the plateau.
-
Uncorrected machine compliance, which inflates early strain and distorts the quasi-elastic gradient and proof strengths.
-
Wrong speed: setting a crosshead speed without converting from strain rate, or changing specimen height without adjusting speed.
-
Not stating the plateau range (20–30 % or 20–40 %) or the upper strain for energy absorption.
-
Underpowered machine: stopping before the plateau end because force rose past capacity during densification.
-
Leaving side stops touching the specimen during the test, which carries load and constrains lateral collapse.
ISO 13314 vs ASTM and related standards
There is no direct ASTM equivalent for compression of porous and cellular metals. The closest methods cover different material classes and should not be substituted:
-
ASTM E9: compression of dense metallic materials at room temperature, aimed at yield and modulus rather than plateau and energy absorption.
-
ASTM D695 and ISO 604: compressive properties of rigid plastics. Similar platen setup, but different specimen rules, speeds and results, and not intended for metals.
-
ISO 844 and ASTM D1621: compression of rigid cellular plastics. These share the foam concept of a compressive stress at a set strain but use plastic-foam specimen sizes and speeds.
-
ISO 17340: the high-speed sister of ISO 13314, covering porous and cellular metals at 0.1 to 100 m/s, used to capture strain-rate effects for crash design.
-
ISO 7500-1 and ISO 9513: the force and extensometer verification standards ISO 13314 references.
-
DIN 50134: a German national method for compression testing of metallic cellular materials; check which standard your customer specifies.
Equipment summary
-
Platens: Universal Grip ISO 13314 hardened compression platens with centring rings and adjustable side stops, 100 kN standard with higher capacities on request. See compression platens.
-
Testing machine: Galdabini benchtop UTMs from 10 kN to 100 kN for most foams and lattices; floor-standing UTMs for large or high-strength specimens; Mark-10 motorized testers for low-force screening.
-
Strain measurement: compliance-corrected crosshead displacement or a video extensometer.
-
Software: testing software for constant-speed control, high-rate data capture and plateau and energy calculations.
-
More: our metals testing page, foam testing page and the full ISO standards hub. Contact us with your specimen size and expected plateau stress for a recommendation.
ISO 13314 FAQ
What is ISO 13314?
ISO 13314 is the ISO test method for the quasi-static compression of porous and cellular metals with a porosity of 50 % or more, such as metal foams and lattice structures. It defines specimen size, test speed and how to determine plateau stress, plateau end and energy absorption.
What is the current edition of ISO 13314?
ISO 13314:2011, the first edition. ISO reviewed and confirmed it in 2022, so it remains current.
How big should an ISO 13314 specimen be?
Every dimension must be at least 10 times the average pore size and at least 10 mm, with a height-to-diameter or height-to-edge ratio between 1 and 2. Cylinders are recommended.
What strain rate does ISO 13314 use?
A constant crosshead speed giving an initial strain rate between 10⁻³ s⁻¹ and 10⁻² s⁻¹. Multiply the strain rate by the specimen height to get crosshead speed.
How is plateau stress defined?
It is the arithmetic mean of the stresses at strain intervals of 0.1 % or smaller between 20 % and 30 %, or 20 % and 40 %, compressive strain. Report which range you used.
What is the plateau end?
The point on the stress-strain curve where the stress reaches 1.3 times the plateau stress. It marks the start of densification.
How is energy absorption calculated?
As the area under the stress-strain curve up to 50 % strain or up to the plateau end strain, in MJ/m³. Efficiency divides that by the maximum stress in the range times the strain range.
How many specimens are required?
At least three, and five are recommended. A preliminary specimen is also used to estimate plateau stress when you need it to set unloading points.
What platens does ISO 13314 require?
Plane-ground, mirror-finished platens with a hardness of at least 60 HRC. Our ISO 13314 platens are hardened tool steel with ground, parallel faces, centring rings and side stops.
Can I use ISO 13314 for 3D-printed lattice structures?
It is widely used for metal lattices because they behave like cellular metals in compression. Check that the specimen contains enough unit cells to satisfy the 10 times pore size rule and state the deviations if not.
Is there an ASTM equivalent to ISO 13314?
Not a direct one. ASTM E9 covers dense metals, and ASTM D695 and ASTM D1621 cover plastics and plastic foams. Use ISO 13314 for porous and cellular metals.
Can a Mark-10 tester run ISO 13314?
For small, low-strength foam specimens a Mark-10 F-series tester up to about 6.7 kN can work for screening. For stronger materials, larger specimens or tests into densification, use a Galdabini universal testing machine.
Need a fixture, grips or a complete test system for ISO 13314? Contact Universal Grip with your material, specimen size and machine connection and we will quote the right setup.