ISO 2439 Indentor Foot for Flexible Foam Hardness Testing by Universal Grip

Downloads: ISO 2439 Indentor Foot for Flexible Foam Hardness Testing – Universal Grip Data Sheet (PDF)

Written by Chris Thomas, Universal Grip Company · Reviewed by Frank Bertini · Updated October 27, 2026

ISO 2439 is the international method for measuring the indentation hardness of flexible foam: the force, in newtons, needed to push a flat 200 mm circular indentor a set percentage into a standard foam block. It is the ISO counterpart of the IFD (indentation force deflection) test in ASTM D3574, and it is the number foam producers, mattress makers, seating suppliers and automotive buyers use to grade how firm a polyurethane or latex foam feels under a body-sized load.

This guide covers the current edition, ISO 2439:2008, in full: all five methods (A to E), the test piece, the indentor and perforated support plate, the preflex cycles, the calculations with worked examples, the rounding rule most reports get wrong, and how ISO 2439 values compare with ASTM D3574 IFD. Universal Grip makes an ISO 2439 indentor foot with a Ø200 mm face, radiused edge and self-aligning spherical seat, with a matching perforated support plate available, for use on your universal testing machine.

In this guide: What ISO 2439 Measures · Current Edition, Scope and Adoptions · Test Pieces: Size, Orientation and Conditioning · Apparatus: Indentor, Support Plate and Testing Machine · Methods A to E at a Glance · Step-by-Step Procedure (Method A) · Calculations and a Worked Example · Interpreting Results and Common Errors · ISO 2439 vs ASTM D3574 IFD and Related Standards · Equipment from Universal Grip · FAQ

What ISO 2439 Measures

ISO 2439 defines indentation hardness as the total force required to produce a specified indentation under specified conditions. The indentation is expressed as a percentage of the test piece thickness, so a 40 % indentation of a 50 mm block means the indentor has travelled 20 mm into the foam from the zero point set by a small preload.

Because the indentor is much smaller than the test piece, the foam around the indentor is drawn down with it. The result is a load-bearing number, not a pure material modulus: it combines the compressive response of the cell structure under the indentor with the shear and tension in the surrounding foam. That is why ISO 2439 values correlate well with how a cushion or mattress feels when someone sits or lies on it.

The standard reports several related values depending on the method:

  • Indentation hardness index (Method A): the force at 40 % indentation after a 30 s hold.

  • Indentation hardness characteristics (Method B): forces at 25 %, 40 % and 65 % indentation, each after a 30 s hold, which describe the shape of the force-indentation curve.

  • Indentation hardness check (Method C): a quick 40 % force with no hold, for quality control.

  • Low indentation hardness index (Method D): the force at 25 % indentation after a 20 s hold, a quick inspection test.

  • Compressive deflection coefficient Sf and hysteresis loss rate Af (Method E): the ratio of the 65 % force to the 25 % force, and the energy lost in one load-unload cycle as a percentage of the loading energy.

Note: ISO 2439 results apply only to the test conditions used. The standard states that they cannot, in general, be used directly for design purposes; use them to compare and specify foams, not to calculate cushion deflection under a given load.

Current Edition, Scope and Adoptions

The current edition is ISO 2439:2008, the fourth edition, published in December 2008 by ISO/TC 45/SC 4. ISO reviewed and confirmed it again in 2026, so it remains current with no amendment. It replaced ISO 2439:1997 and its 1998 corrigendum. The 1997 edition contained only Methods A, B and C; the 2008 edition added Method D and Method E.

In Europe it is published as EN ISO 2439:2008, with national adoptions such as BS EN ISO 2439 and DIN EN ISO 2439, all technically identical to the ISO text.

The scope is narrower than many summaries suggest. The five methods apply only to open-cell latex foam, urethane (polyurethane) foam and PVC foam. Closed-cell sponge and rigid foams are outside the scope; rigid cellular plastics are tested in compression to ISO 844 instead. ISO 2439 can be used on bulk material cut to the standard size and on finished articles such as cushions and mattresses, but results on finished articles or plied material can differ from those on the standard test piece.

Test Pieces: Size, Orientation and Conditioning

The standard test piece is a square block of foam with a thickness of 50 mm. Key requirements:

  • Shape: square, side length 380 mm.

  • Thickness: 50 ± 2 mm.

  • Thin sheet: plies may be stacked to approximate the standard thickness; record the number of plies.

  • Skins: record whether the piece has moulded or cut skins and how many; skin stiffens the result.

  • Orientation: if the foam has a rise direction or oriented cells, test in the direction agreed between the parties, normally the direction in which the product is loaded in service.

  • Finished articles: may be tested as supplied, centred under the indentor; a moulded article with cavities is placed with the cavity side against the support plate.

Fresh foam continues to cure and its hardness changes during the first days. ISO 2439 therefore says material shall not be tested less than 72 h after manufacture, unless it has been shown that results at 16 h or 48 h are within ±10 % of the 72 h result, in which case the shorter time is allowed. For quality-control tests, pieces may be taken as early as 12 h after manufacture.

Before testing, condition the test pieces for at least 16 h in one of the standard atmospheres of ISO 23529: 23 ± 2 °C and 50 ± 5 % relative humidity, or 27 ± 2 °C and 65 ± 5 % relative humidity. Quality-control tests allow a minimum of 6 h conditioning. Test in the same atmosphere, because flexible polyurethane foam hardness is sensitive to both temperature and humidity.

Apparatus: Indentor, Support Plate and Testing Machine

Indentor

The indentor is a flat, rigid, circular plate 200 mm in diameter (the tolerance allows up to 203 mm), with a small radius of about 1 mm on its lower edge so it does not cut the foam. The lower face is smooth but not polished. The standard prefers a ball-jointed mounting so the indentor can align itself with the top face of the test piece; a fixed indentor that meets the foam at an angle loads one side first and reads high.

Support plate

The test piece sits on a smooth, flat, horizontal, rigid support that is larger than the test piece. It must be perforated with vent holes of about 6 mm diameter at about 20 mm pitch. Without the holes, air trapped under an open-cell block acts as a cushion and the measured force rises, especially at 65 % indentation.

Testing machine and force measurement

  • Drive: the indentor moves vertically at 100 ± 20 mm/min for all loading and unloading.

  • Force accuracy: ISO 7500-1 Class 1, or within ±1 N.

  • Thickness measurement under the preload: to ±0.25 mm.

  • Position control: the machine must hold the indentation constant to within ±0.25 mm during each hold period.

  • Methods C and E: a peak-hold (tell-tale) force indicator or a recording of the full force-indentation curve.

A modern universal testing machine with displacement control and a load cell sized for foam does all of this. Typical indentation forces for seating and bedding foams run from tens to a few hundred newtons, so choose a load cell whose Class 1 range covers both the low 25 % values and the 65 % peak. Also check the frame geometry: the support plate is wider than a 380 mm block, so the clearance between the columns, or the throat of a single-column frame, must accept it.

Methods A to E at a Glance

All five methods start the same way: centre the test piece on the support plate under the indentor, apply a preload of about 5 N, and record the thickness under that preload as the zero point. Every indentation percentage is calculated from that thickness. The methods then differ in preflex, target indentation and hold time:

  • Method A, 40 %/30 s index: 3 preflex cycles to 70 ± 2.5 %; indent to 40 ± 1 %; hold 30 ± 1 s; read force. Laboratory reference method.

  • Method B, 25 %-40 %-65 %/30 s characteristics: 3 preflex cycles to 70 ± 2.5 %; indent in steps to 25 ± 1 %, 40 ± 1 % and 65 ± 1 %; hold 30 ± 1 s at each; read force at the end of each hold.

  • Method C, 40 % check: 3 preflex cycles to 70 ± 2.5 %; indent to 40 ± 1 %; read force immediately, with no hold. Quality-control method.

  • Method D, 25 %/20 s low index: 1 preflex cycle to 75 ± 2.5 %; indent to 25 ± 1 %; hold 20 ± 1 s; read force. Quick inspection method.

  • Method E, Sf and hysteresis: 1 preflex cycle to 75 ± 2.5 %; rest 4 ± 1 min; one recorded cycle to 75 ± 2.5 % and back, reversing within 2 s; compute Sf and Af from the curve.

Note: Method D holds for 20 s, not 30 s. Several published summaries list it as 25 %/30 s; the ISO title of Method D is the 25 %/20 s low indentation hardness index.

Annex A of the standard summarizes these parameters and shows a typical force-indentation graph for each method.

Step-by-Step Procedure (Method A)

Method A is the reference method and the one most specifications quote. A typical run on a 50 mm block looks like this:

  • 1. Confirm the test piece is at least 72 h old (or meets the 16 h/48 h or quality-control exceptions) and has been conditioned for at least 16 h.

  • 2. Fit the 200 mm indentor and the perforated support plate. Check the indentor face is parallel to the support and free to self-align.

  • 3. Centre the test piece under the indentor, cavity side down for moulded articles.

  • 4. Lower the indentor to a preload of about 5 N and record the thickness, for example 50.0 mm. This is the zero point.

  • 5. Preflex: indent to 70 % (35.0 mm of travel) and return, three times, at 100 ± 20 mm/min. This breaks in the cell structure so the measurement reflects the working foam, not its as-made stiffness.

  • 6. Immediately after the third unloading, indent to 40 % (20.0 mm) at 100 ± 20 mm/min.

  • 7. Hold the position for 30 ± 1 s, keeping the indentation within ±0.25 mm. The force falls during the hold as the foam relaxes.

  • 8. Record the force at the end of the hold. This is the 40 %/30 s indentation hardness index.

  • 9. Return the indentor and remove the test piece.

Method B follows steps 1 to 6 and then holds at 25 %, 40 % and 65 % in turn. Method C stops at step 6 and reads the peak force. Methods D and E use the single 75 % preflex cycle described above.

If you need to retest the same test piece, ISO 2439 requires a recovery of at least 16 h first. Retesting a block minutes after a run gives a low value because the cells have not fully recovered.

Calculations and a Worked Example

Method A and B forces

Method A and B results are read directly as forces in newtons. Method B also gives two indentation factors: the 25 % force divided by the 40 % force, and the 65 % force divided by the 40 % force.

Worked example, Method B on a 50.0 mm thick test piece (thickness measured under the preload):

  • Indentations: 25 % = 12.5 mm, 40 % = 20.0 mm, 65 % = 32.5 mm.

  • Measured forces after 30 s holds: F25 = 98 N, F40 = 140 N, F65 = 285 N.

  • Factor F25/F40 = 98 ÷ 140 = 0.70.

  • Factor F65/F40 = 285 ÷ 140 = 2.04.

Rounding rule

ISO 2439 asks for indentation values up to 100 N to be rounded to the nearest 1 N, and values above 100 N to the nearest 5 N. A Method A reading of 152 N is therefore reported as 150 N, and 98 N stays 98 N. Many lab reports quote 152 N, which implies precision the method does not have.

Method E: Sf and Af

The compressive deflection coefficient is Sf = F65 ÷ F25, where both forces are taken from the loading curve of the recorded cycle. The hysteresis loss rate is Af = (area of the hysteresis loop ÷ area under the loading curve) × 100 %.

  • Recorded cycle: F25 = 105 N, F65 = 260 N, so Sf = 260 ÷ 105 = 2.48.

  • Area under the loading curve (energy input) = 6.20 J; area enclosed by the loop (energy lost) = 1.55 J.

  • Af = 1.55 ÷ 6.20 × 100 = 25.0 %.

Annex B of the standard gives precision data for Method E.

Interpreting Results and Common Errors

The 40 % index is the headline firmness grade. Sf (or the 65/25 ratio from Method B) describes how quickly the foam stiffens as it is compressed: a higher value means the foam feels soft on first contact but supports well at depth, which is desirable in seating. Af describes how much energy the foam absorbs per cycle; high-resilience foams have lower hysteresis loss than conventional or viscoelastic foams.

Errors that move ISO 2439 results most:

  • Wrong zero point: measuring thickness under too high a preload, or from a crosshead position, shifts every indentation percentage.

  • Skipping or shortening the preflex: unflexed foam reads noticeably harder.

  • Wrong speed: running Method A at an ASTM-style 50 mm/min or 250 mm/min changes the force; ISO uses 100 ± 20 mm/min throughout.

  • Hold time and drift: reading the force at the start of the hold instead of the end, or letting the crosshead creep, changes the result. Method C has no hold and reads higher than Method A for the same foam.

  • Unperforated or undersized support: trapped air adds force; a support smaller than the test piece lets the edges sag.

  • Fixed, misaligned indentor: one edge contacts first and the curve shows a false toe.

  • Fresh or unconditioned foam: testing a block a few hours after production, or straight from a cold or humid warehouse.

  • Retesting too soon: less than 16 h recovery on the same piece.

  • Mixing methods: Method A, C and D values are not interchangeable, and plied or finished-article results are not equal to standard-piece results.

ISO 2439 vs ASTM D3574 IFD and Related Standards

The closest ASTM method is Test B1 (indentation force deflection) of ASTM D3574, whose current edition is D3574-25. Both use a 200 mm circular indentor on a perforated support plate, but the procedures differ enough that ISO and ASTM numbers must never be compared directly:

  • Standard test piece: ISO 380 mm square × 50 mm thick; ASTM at least 380 × 380 × 100 mm.

  • Preload: ISO about 5 N; ASTM 4.5 N.

  • Preflex: ISO three cycles to 70 % at 100 mm/min; ASTM two cycles to 75–80 % at 250 mm/min, then a 6 min rest.

  • Indentation speed: ISO 100 mm/min; ASTM 50 mm/min.

  • Hold time: ISO 30 s (20 s for Method D); ASTM 60 s.

  • Indentation levels: ISO 40 % headline value; ASTM 25 % and 65 % IFD.

  • Ratio: ISO Sf = F65/F25 (Method E); ASTM support factor = 65 % IFD ÷ 25 % IFD.

Thickness alone changes the answer: a 100 mm block indented 25 % travels 25 mm, a 50 mm block only 12.5 mm, and the surrounding foam is drawn down differently. Convert between the two only with a correlation built on your own foam.

Related flexible foam methods often specified alongside ISO 2439:

  • ISO 1856: compression set of flexible foam, the companion durability test.

  • ISO 3386-1: compression stress-strain characteristics of whole-face compression, where the platen covers the full test piece.

  • ISO 1798: tensile strength and elongation of flexible foam.

  • ISO 8067: tear strength of flexible foam.

  • ISO 845: apparent density, which should accompany every hardness value.

  • ISO 23529: conditioning atmospheres; ISO 7500-1: force verification of the testing machine.

Equipment from Universal Grip

ISO 2439 indentor foot (part ref. UGC-ISO2439-CP)

Our ISO 2439 fixture is a circular indentor foot for indentation hardness testing of flexible foam. The flat foot with a radiused edge presses into the foam test piece, a bolted spherical seat lets it self-align to the specimen surface, and a pin connection mounts it directly to the load cell.

  • Contact surface: flat Ø200 mm indentor face with radiused edge, per ISO 2439 geometry.

  • Alignment: bolted spherical seat.

  • Construction: rigid steel foot with a corrosion-resistant finish for uniform indentation across the face.

  • Load capacity: 5 kN standard; higher capacities on request.

  • Machine connection: pin connection or threaded adapter, to suit your frame.

  • Support: a matching perforated support plate is available.

  • Applications: flexible polyurethane foam, latex foam, mattresses, seating and automotive cushions, and foam production QC.

When ordering, tell us the indentor diameter you need, whether you need the support plate, and your test machine connection. The same frame can also run ASTM D3574 work with the appropriate fixtures; see our foam testing page and our range of compression fixtures.

Machines, software and adapters

ISO 2439 needs displacement-controlled cycling, timed holds and curve recording for Method E, so pair the indentor with one of our universal testing machines and testing software that can program preflex, hold and readout steps. Adapters are available to connect the indentor to other frames. For a quote on any of these, contact us.

ISO 2439 FAQ

What is ISO 2439?

ISO 2439 is the international standard for determining the indentation hardness of flexible cellular materials such as polyurethane and latex foam. A flat 200 mm circular indentor is pushed into a 50 mm thick foam block and the force at a set indentation is recorded in newtons. The current edition is ISO 2439:2008.

What is the current edition of ISO 2439?

The current edition is ISO 2439:2008, the fourth edition, published in December 2008. ISO confirmed it again in 2026, so it remains current with no amendments. It is adopted in Europe as EN ISO 2439:2008.

What is the difference between ISO 2439 Methods A, B, C, D and E?

Method A gives the 40 %/30 s indentation hardness index; Method B records forces at 25 %, 40 % and 65 % with 30 s holds; Method C is a quick 40 % check with no hold; Method D is a quick 25 %/20 s low index; Method E gives the compressive deflection coefficient Sf and the hysteresis loss rate. Methods A, B and C use three preflex cycles to 70 %, while D and E use one cycle to 75 %.

What size test piece does ISO 2439 use?

The standard test piece is a square 380 mm on a side with a thickness of 50 ± 2 mm. Thinner material can be plied to approximate 50 mm, and finished articles can be tested, but those results may differ from standard-piece values. Record the thickness, plies and skins in the report.

What indentor does ISO 2439 require?

A flat, rigid circular indentor 200 mm in diameter (up to 203 mm within tolerance), with a small radius of about 1 mm on the lower edge and a smooth, unpolished face. A ball-jointed or spherical-seat mounting is preferred so it aligns with the foam. Universal Grip's ISO 2439 indentor foot has a Ø200 mm face, radiused edge and bolted spherical seat.

What test speed does ISO 2439 use?

All loading and unloading in ISO 2439 is at 100 ± 20 mm/min. This differs from ASTM D3574 Test B1, which preflexes at 250 mm/min and indents at 50 mm/min, one reason the two standards give different numbers.

Why does ISO 2439 require preflexing?

New foam has some closed or partly bonded cell windows that make it read stiffer on the first compression. Three cycles to 70 % (Methods A to C) or one to 75 % (Methods D and E) break the foam in, so the measured force reflects the foam as it behaves in use and results repeat between labs.

How do I calculate the compressive deflection coefficient and hysteresis loss?

Sf is the force at 65 % indentation divided by the force at 25 %, both from the loading curve of the Method E cycle; for example 260 N ÷ 105 N = 2.48. The hysteresis loss rate is the area of the load-unload loop divided by the area under the loading curve, times 100; 1.55 J ÷ 6.20 J gives 25.0 %.

How should ISO 2439 results be rounded?

Indentation values up to 100 N are rounded to the nearest 1 N, and values above 100 N to the nearest 5 N. So 98 N is reported as 98 N, but 152 N is reported as 150 N.

Can I convert ISO 2439 hardness to ASTM D3574 IFD?

Not with a fixed factor. ISO 2439 uses a 50 mm thick piece, 100 mm/min, a 70 % preflex and 30 s holds, while ASTM D3574 Test B1 uses a 100 mm piece, 50 mm/min indentation, a 75–80 % preflex and 60 s holds. Build a correlation by testing your own foams to both standards.

How long after manufacture can foam be tested to ISO 2439?

Not sooner than 72 h after manufacture, unless results at 16 h or 48 h have been shown to be within ±10 % of the 72 h result. Quality-control tests may sample as early as 12 h with at least 6 h conditioning. Standard conditioning is at least 16 h at 23 °C and 50 % RH, or 27 °C and 65 % RH.

Can the same foam block be retested?

Yes, but ISO 2439 requires at least 16 h of recovery before a repeat test on the same test piece. Retesting sooner gives low values because the foam has not fully recovered from the previous cycles.

Need a fixture, grips or a complete test system for ISO 2439? Contact Universal Grip with your material, specimen size and machine connection and we will quote the right setup.

bottom of page