top of page

ISO 1856
Compression Set of Flexible Foam

ISO 1856 Compression Set Clamping Device for Flexible Foam by Universal Grip

Downloads: ISO 1856 Compression Set Clamping Device for Flexible Foam – Universal Grip Data Sheet (PDF)

Written by Chris Thomas, Universal Grip Company · Reviewed by Frank Bertini · Updated October 27, 2026

ISO 1856 is the international test for compression set of flexible foam: how much thickness a latex or polyurethane foam permanently loses after being held squashed for a set time at a set temperature. A 25 mm thick test piece is clamped between flat plates at 50 % or 75 % deflection, typically for 22 h at 70 °C, then released and measured after 30 minutes of recovery. The loss of thickness, as a percentage of the original thickness, is the compression set.

Foam producers, mattress and furniture makers, automotive seating suppliers and packaging engineers use ISO 1856 to screen foam durability and to accept material against specifications. This guide covers the current edition, ISO 1856:2018, step by step, with test piece rules, spacer selection, a worked five-piece example and the differences from ASTM D3574 Test D. Universal Grip builds a multi-level ISO 1856 clamping device that holds test pieces at fixed deflection inside a laboratory ageing oven, with no load frame needed.

In this guide: What ISO 1856 Measures · Current Edition, Scope and Changes · Test Pieces: Size, Number and Conditioning · Apparatus: Compression Device, Spacers and Oven · Method A, B or C: Which to Use · Step-by-Step Procedure (Method A) · Calculation and Worked Example · Interpreting Results and Common Errors · ISO 1856 vs ASTM D3574 Test D and Related Standards · Equipment from Universal Grip · FAQ

What ISO 1856 Measures

ISO 1856 defines compression set as the difference between the initial thickness and the final thickness of a test piece after it has been compressed for a given time at a given temperature and then allowed to recover for a given time, with that difference referred to the initial thickness. In plain terms: how much of its height the foam fails to recover.

The principle is constant deflection, not constant load. The test piece is squeezed to a fixed height by spacers between two plates and held there, so the force in the foam is free to relax during the test. Heat accelerates the physical and chemical changes in the polymer network that make a cushion or seal take a permanent set in service, so a day at 70 °C stands in for a much longer period of use.

A low result means good recovery; a high result means the foam will bottom out, lose loft or leave a permanent body impression in use. Compression set is one of the most frequently specified durability properties for seating foam, mattress layers and foam gaskets.

Current Edition, Scope and Changes

The current edition is ISO 1856:2018, the fourth edition, published in June 2018 by ISO/TC 45/SC 4 and confirmed by ISO in 2024, so it remains current. It replaced ISO 1856:2000 and incorporates that edition's Amendment 1 of 2007. In Europe it is EN ISO 1856:2018, with national adoptions such as BS EN ISO 1856:2018 and DIN EN ISO 1856.

The 2018 edition made these changes:

  • Added ISO 23529 (conditioning of test pieces) as a normative reference.

  • Added a further requirement for test pieces in clause 6.1.

  • Amended the conditioning rules in clause 6.4.

  • Added temperature tolerances for Methods A and B.

  • Incorporated Amendment 1:2007.

Scope: ISO 1856 specifies three methods, A, B and C, and currently applies only to latex and polyurethane foams of thickness greater than 2 mm. Solid vulcanized and thermoplastic rubber is tested to ISO 815-1 instead, and closed-cell sponge rubber is commonly tested to ASTM D1056.

Test Pieces: Size, Number and Conditioning

  • Size: 50 ± 1 mm long × 50 ± 1 mm wide × 25 ± 1 mm thick.

  • Faces: top and bottom parallel, sides essentially vertical.

  • Condition: free from contamination, with no skin on the vertical sides.

  • Number: five test pieces, or five assemblies for thin material.

  • Orientation: compress in the direction in which the finished product is stressed in service.

Thin materials

Foam thinner than 25 mm, down to the 2 mm scope limit, is tested as an assembly: 50 mm × 50 mm plies stacked to a total thickness of at least 25 mm before compression, using a minimum of two plies. When there are more than two plies, glass mounting slides 1 to 1.5 mm thick and 50 to 55 mm square are interleaved between them. The slide thickness is subtracted when measuring the foam thickness, and the assembly is treated as a single test piece.

Age and conditioning

Materials shall not be tested less than 72 h after manufacture, unless it has been shown that results after 16 h or 48 h are within ±10 % of the 72 h results, in which case testing is allowed at 16 h or 48 h. Condition the test pieces for at least 16 h in one of these atmospheres:

  • 23 ± 2 °C and 50 ± 5 % relative humidity, or

  • 27 ± 2 °C and 65 ± 5 % relative humidity.

For quality-control testing, test pieces can be taken sooner, down to 12 h after manufacture, with a minimum of 6 h conditioning. Record which atmosphere and which ages you used; both appear in the test report.

Apparatus: Compression Device, Spacers and Oven

ISO 1856 does not use a testing machine. The required apparatus is simple but has to be right:

  • Compression device: two flat plates larger than the test pieces, with spacers and clamps that hold the plates parallel at the required deflected height.

  • Spacers: sized so the gap between the plates equals the compressed thickness of the test piece.

  • Thickness gauge: measurement of linear dimensions to ISO 1923.

  • Oven: able to hold 70 ± 1 °C for Method A; a circulating-air oven helps every level of a multi-level clamp reach temperature.

  • Recovery surface: a material of low thermal conductivity, such as wood, at the conditioning temperature.

Choosing spacer height

ISO 1856 compresses the test piece by a percentage of its thickness, so the spacer height equals the remaining thickness:

  • 50 % compression of a 25.0 mm test piece: spacer 12.5 mm.

  • 75 % compression of a 25.0 mm test piece: spacer 6.25 mm.

  • 90 % compression, by special agreement: spacer 2.5 mm.

The standard allows a tolerance of ±4 percentage points on the 50 % and 75 % levels, so a spacer does not have to be exact for every piece within the 25 ± 1 mm thickness band. For example, a 12.7 mm spacer compresses a 25.0 mm piece by (25.0 − 12.7) ÷ 25.0 = 49.2 %, and a 24.0 mm piece by 47.1 %, both inside 50 ± 4 %. Always calculate the actual deflection from the measured thickness and choose spacers that keep every piece inside the band.

With a multi-level clamp, every level must be set to its own spacer height and every plate must seat fully on its spacers before the device goes into the oven. A plate that rests on the foam instead of the spacers applies a load, not a fixed deflection, and that level's results are invalid.

Note: Compressed by 75 % means the foam is squeezed to 25 % of its thickness, not to 75 %. Mixing up the two is the most common set-up error in compression set testing.

Method A, B or C: Which to Use

The test may be carried out by Method A, Method B, Method C, or all three. The methods do not necessarily give the same results, so a specification must name the method and conditions.

  • Method A, compression at 70 °C: (50 ± 4) % or (75 ± 4) % compression, 22 ± 0.2 h in an oven at 70 ± 1 °C. The default, most widely specified condition.

  • Method B, compression at the standard conditioning temperature: same deflection, held for 72 h at the conditioning temperature (23 °C or 27 °C), within the tolerance given in the standard. Simulates long static loading at room temperature without heat acceleration.

  • Method C, specially specified conditions: the time, temperature and degree of compression are agreed between the interested parties, for example a different temperature, a longer duration, or 90 % compression.

Method C is also how specifications add conditions ISO 1856 does not fix, such as a different ageing temperature, a longer hold or 90 % compression. Some specifications also measure compression set after accelerated humid ageing to ISO 2440; the ageing conditions then come from the specification, while the compression and thickness measurement follow ISO 1856. Whatever the conditions, write them after the result so the value can be compared with others.

Most foam purchase specifications call for Method A at 50 % or 75 % compression. Higher compression levels are more severe and give higher set values, so a value quoted without its compression level is meaningless.

Step-by-Step Procedure (Method A)

  • 1. Cut five test pieces to 50 × 50 × 25 mm, check age after manufacture, and condition them for at least 16 h.

  • 2. Measure the initial thickness d0 of each piece to ISO 1923 at the conditioning atmosphere.

  • 3. Select spacers that give (50 ± 4) % or (75 ± 4) % compression for the measured thicknesses.

  • 4. Place the test pieces between the plates, centred and spaced apart so they do not touch each other or the tie rods when they bulge under compression.

  • 5. Tighten the clamp evenly until the plates seat on the spacers, keeping the plates parallel.

  • 6. Within 15 min of compressing, put the loaded device in the oven at 70 ± 1 °C.

  • 7. Leave it for 22 ± 0.2 h.

  • 8. Remove the device from the oven and, within 1 min, release the test pieces and place them on a low-conductivity surface such as wood.

  • 9. Allow 30 ± 5 min recovery at the conditioning temperature.

  • 10. Measure the final thickness dr of each piece at the same location as d0.

  • 11. Calculate compression set for each piece and report all five values and the median.

Method B follows the same sequence with the device left for 72 h at the conditioning temperature instead of in the oven. Thin-material assemblies should be handled without disturbing the plies during release and remeasurement.

Calculation and Worked Example

Compression set, in percent, is:

Compression set = (d0 − dr) ÷ d0 × 100

  • d0: initial thickness of the test piece, mm.

  • dr: thickness after recovery, mm.

Worked example, Method A, 50 % compression, 22 h at 70 °C, five test pieces:

  • Piece 1: d0 = 25.2 mm, dr = 23.7 mm, set = 1.5 ÷ 25.2 × 100 = 6.0 %.

  • Piece 2: d0 = 24.8 mm, dr = 23.4 mm, set = 1.4 ÷ 24.8 × 100 = 5.6 %.

  • Piece 3: d0 = 25.0 mm, dr = 23.6 mm, set = 1.4 ÷ 25.0 × 100 = 5.6 %.

  • Piece 4: d0 = 25.1 mm, dr = 23.5 mm, set = 1.6 ÷ 25.1 × 100 = 6.4 %.

  • Piece 5: d0 = 24.9 mm, dr = 23.6 mm, set = 1.3 ÷ 24.9 × 100 = 5.2 %.

Ranked, the values are 5.2, 5.6, 5.6, 6.0 and 6.4 %, so the median is 5.6 %. ISO 1856 reports the result followed by the test conditions in brackets in the order compression, time, temperature: 5.6 % (50 %, 22 h, 70 °C). The mean of the five values, 5.8 %, is not the reported result.

Note that ISO 1856 always refers the loss to the original thickness. It does not express set as a percentage of the applied deflection, which would give a value twice as large at 50 % compression.

Interpreting Results and Common Errors

There is no pass mark in ISO 1856 itself; limits come from product specifications. As a rough guide, good polyurethane and latex seating foams show single-digit compression set at 50 %, 22 h, 70 °C, while values in the tens of percent point to poor cure, unsuitable chemistry or degraded material. Compare foams only at identical method, compression level, time and temperature.

Errors that most often distort results:

  • Compressing to the percentage instead of by it, or using the wrong spacer for the measured thickness.

  • Plates that are not parallel, so one side of each piece is over-compressed.

  • Pieces too close together, or against the tie rods, so bulging foam is pinched or restrained.

  • Plates smaller than the test pieces, so edges are not compressed at all.

  • Slow loading into the oven, more than 15 min after compression, or an oven that is opened repeatedly.

  • Releasing pieces late after removal from the oven, or recovering them on a cold metal bench instead of wood.

  • Measuring too early or too late: recovery is 30 ± 5 min, not 'up to an hour'. Foam keeps recovering, so a late reading gives a lower set.

  • Testing fresh foam less than 72 h after manufacture without the validated exception.

  • Skin left on vertical sides, which restrains bulging and recovery.

  • Reporting the mean instead of the median, or omitting the conditions after the value.

ISO 1856 vs ASTM D3574 Test D and Related Standards

The ASTM counterpart is Test D, constant deflection compression set, in ASTM D3574, whose current edition is D3574-25. The tests look alike, but the details differ:

  • Test piece: both 50 × 50 × 25 mm.

  • Number: ISO five pieces, median reported; ASTM three specimens.

  • Compression: ISO (50 ± 4) % or (75 ± 4) %, 90 % by agreement; ASTM 50, 75 or 90 % within ±1 %.

  • Heat ageing: ISO 22 ± 0.2 h at 70 ± 1 °C; ASTM 22 h at 70 ± 2 °C.

  • Recovery: ISO 30 ± 5 min; ASTM 30 to 40 min.

  • Room-temperature option: ISO Method B holds 72 h at the conditioning temperature; check your ASTM specification for any equivalent condition.

  • Calculation: ISO uses original thickness only; ASTM offers Ct, based on original thickness, as the default and Cd, based on the deflection, as an alternative.

ISO 1856 results and ASTM Ct values at the same compression, time and temperature measure the same quantity, but the different tolerances, specimen count and recovery window mean they are not formally interchangeable; a specification should name one standard. Cd values are always larger and must never be compared with ISO 1856 results.

Related standards:

  • ISO 2439: indentation hardness of flexible foam, normally reported alongside compression set.

  • ISO 815-1 and ASTM D395: compression set of solid vulcanized and thermoplastic rubber.

  • ISO 1923: measurement of linear dimensions of cellular plastics and rubbers.

  • ISO 23529: preparation and conditioning of test pieces.

Equipment from Universal Grip

ISO 1856 compression set clamping device (part ref. UGC-ISO1856-CP)

Our ISO 1856 fixture is a multi-level clamping device for compression set testing of flexible foam. Foam test pieces are stacked between flat steel plates separated by spacer bars of set height, and tie rods with nuts clamp the stack down to the spacers, holding each level at a fixed compression during ageing. It is an oven clamp, not a set of load-frame platens: once tightened, it goes straight into the ageing oven.

  • Test method: compression set at constant deflection, fixed-deflection bolted clamp.

  • Plates: flat, parallel steel plate faces that compress foam evenly across the test piece.

  • Compression: set by spacer height, with spacers made to suit your test piece thickness and compression percentage.

  • Levels: several levels test multiple specimens or thicknesses at once.

  • Construction: steel plates and tie rods with a corrosion-resistant finish.

  • Size: compact frame, approx. 203 mm wide × 176 mm high per drawing, to fit laboratory ageing ovens.

  • Use: bench and oven use; no load frame required.

  • Applications: flexible polyurethane foam, latex and rubber foams, seating, bedding and packaging foams, and durability and ageing studies.

When ordering, specify the test piece size and thickness, the compression percentage, the number of levels and the maximum ageing temperature. For foam that will be checked for hardness as well, our ISO 2439 indentor foot runs on a universal testing machine; see our foam testing and compression fixtures pages, and our environmental chambers for elevated-temperature work. For a quote, contact us.

ISO 1856 FAQ

What is ISO 1856?

ISO 1856 is the international standard for determining the compression set of flexible cellular polymeric materials, specifically latex and polyurethane foams over 2 mm thick. A test piece is held at a fixed deflection for a set time and temperature, released, and its loss of thickness is expressed as a percentage of the original thickness.

What is the current edition of ISO 1856?

The current edition is ISO 1856:2018, the fourth edition, published in June 2018 and confirmed by ISO in 2024. It replaced ISO 1856:2000 and its 2007 amendment, and is adopted in Europe as EN ISO 1856:2018.

What are the standard ISO 1856 test conditions?

Method A compresses the foam by 50 % or 75 % (±4 %) for 22 h in an oven at 70 ± 1 °C, followed by 30 ± 5 min recovery at the conditioning temperature. Method B holds the same deflection for 72 h at the conditioning temperature, and Method C uses agreed conditions.

What size are ISO 1856 test pieces?

Test pieces are 50 ± 1 mm × 50 ± 1 mm × 25 ± 1 mm with parallel faces and no skin on the vertical sides. Five test pieces are tested. Material thinner than 25 mm is plied, at least two plies, to a total of 25 mm or more.

How is ISO 1856 compression set calculated?

Compression set = (d0 − dr) ÷ d0 × 100, where d0 is the initial thickness and dr is the thickness after recovery. For example, a 25.0 mm piece that recovers to 23.6 mm has a compression set of 1.4 ÷ 25.0 × 100 = 5.6 %. Report the median of five pieces with the conditions, such as 5.6 % (50 %, 22 h, 70 °C).

What spacer height do I need for 50 % or 75 % compression?

Spacer height equals the compressed thickness. For a 25.0 mm test piece, 50 % compression needs a 12.5 mm spacer and 75 % compression a 6.25 mm spacer. Check each piece's measured thickness, because the deflection must stay within ±4 percentage points of the target.

How long is the recovery time in ISO 1856?

30 ± 5 minutes at the conditioning temperature, on a low thermal conductivity surface such as wood. The pieces must be released within 1 minute of removing the device from the oven. Measuring after an hour, as some summaries suggest, gives a lower and non-compliant result.

What is the difference between ISO 1856 and ASTM D3574 Test D?

Both use 50 × 50 × 25 mm pieces and 22 h at 70 °C, but ISO tests five pieces and reports the median, allows ±4 % on compression, holds 70 ± 1 °C and recovers 30 ± 5 min. ASTM D3574 Test D uses three specimens, ±1 % compression, 70 ± 2 °C and 30 to 40 min recovery, and offers a deflection-based Cd value that ISO does not use.

Is ISO 1856 the same as ISO 815-1?

No. ISO 1856 covers flexible latex and polyurethane foam, while ISO 815-1 covers solid vulcanized and thermoplastic rubber with different test piece sizes and compression levels. Their results are not comparable.

Do I need a testing machine for ISO 1856?

No. ISO 1856 uses a clamping device of flat plates, spacers and clamps placed in an oven, plus a thickness gauge. Universal Grip's ISO 1856 clamping device uses tie rods and nuts to clamp several levels of test pieces to the spacer height without a load frame.

What is a good compression set value for foam?

ISO 1856 sets no limit; acceptance values come from product specifications. Lower is better, and good seating and bedding foams generally show single-digit values at 50 %, 22 h, 70 °C. Always compare results at the same method, compression, time and temperature.

How soon after manufacture can foam be tested?

Not less than 72 h after manufacture, unless results at 16 h or 48 h have been shown to be within ±10 % of the 72 h result. Quality-control tests may sample from 12 h with at least 6 h conditioning. Normal conditioning is at least 16 h at 23 °C and 50 % RH or 27 °C and 65 % RH.

Need a fixture, grips or a complete test system for ISO 1856? Contact Universal Grip with your material, specimen size and machine connection and we will quote the right setup.

bottom of page