ASTM F88 is the standard seal strength test for flexible packaging: a 25 mm (1 in) strip cut across a heat seal is pulled apart in a tensile tester, and the force needed to open the seal is reported per unit width. It looks like the simplest test in a packaging lab, and it is one of the easiest to get wrong. The same seal reads differently depending on how the tail is held (Technique A, B or C), how the strip is cut, where the seal sits between the jaws, which part of the force trace you average, and whether a hose is dragging on the crosshead. This complete guide covers the three techniques, strip width and cutting, conditioning, the 200 to 300 mm/min test speed, which testing machine to use (a Mark-10 tensile tester or a Galdabini universal testing machine), grips, whether you need an extensometer (you do not), failure modes, the calculation with a worked example, F88 vs. EN 868-5 and ASTM F2824, troubleshooting and a full FAQ, with setup videos from our lab.

For the standard reference page and fixture options, see our ASTM F88 seal strength test page. This article focuses on how to set up and run the test, how to read the result and which equipment to choose.

ASTM F88 at a glance

  • Full title: Standard Test Method for Seal Strength of Flexible Barrier Materials (published as F88/F88M; the current edition at the time of writing is F88/F88M-23).

  • What it measures: the force needed to separate a strip that contains a seal, and the mode of failure. Results are reported as force per unit width, in N/25 mm, N/15 mm or lbf/in.

  • Seal types covered: flexible-to-flexible seals (film to film, film to Tyvek or paper) and flexible-to-rigid or semi-rigid seals (lidding to a tray flange).

  • Specimens: strips cut perpendicular to the seal, 25 mm, 15 mm or 25.4 mm (1.00 in) wide, with tails long enough to grip.

  • Techniques: A unsupported tail, B tail supported at 90° by hand, C supported at 180° with the less flexible tail held flat against an alignment plate. Use one technique for a whole test series and report it.

  • Test speed: a constant rate of grip separation of 200 to 300 mm/min (8 to 12 in/min); 250 mm/min (10 in/min) is a common choice.

  • Primary result: maximum seal strength (peak force ÷ width). Average seal strength over the peel may also be reported, with the averaging method stated.

  • Failure mode: recorded for every specimen (peel at the seal interface, delamination, tear or break of the material, elongation and so on).

  • Typical forces: a few newtons to a few tens of newtons per strip, so a low-capacity load cell matters more than frame capacity.

  • Typical equipment: a Mark-10 tensile tester or Galdabini universal testing machine, rubber-faced pneumatic grips or vise grips, a precision strip cutter, and an alignment plate for Technique C.

What ASTM F88 measures and who uses it

A package seal has two jobs that pull in opposite directions. It must be strong enough to survive sterilization, shipping and handling without opening, and for peelable packaging it must open cleanly with a reasonable hand force and without tearing the material or shedding fibres. F88 puts a number on both. A minimum seal strength shows the seal will hold; an upper limit shows a peelable pouch or lid will open without a struggle.

Because it is quick, cheap and quantitative, F88 is used throughout the packaging life cycle:

  • Medical device and pharmaceutical packaging: pouches, header bags and trays sealed with Tyvek, paper or film lidding. ISO 11607-1 requires seal strength to be specified and validated, and F88 is the method most often cited, before and after sterilization and aging.

  • Process validation and control: a seal curve (strength against seal temperature, dwell and pressure) sets the sealing window, and routine F88 testing keeps the sealer inside it.

  • Food and consumer packaging: snack bags, retort pouches, stick packs, lidded cups and blisters.

  • Material development: comparing sealants, coatings, laminates and heat-seal lacquers.

F88 tests a strip, not a package. A seal can pass F88 and still leak through a channel or pinhole, so F88 is used alongside integrity tests such as dye penetration (ASTM F1929), bubble leak (ASTM F2096) and whole-package burst (ASTM F1140 and F2054). For lids peeled from round containers, ASTM F2824 applies instead.

The three test techniques: A, B and C

The biggest source of disagreement in F88 data is the angle at which the tail is held while the seal opens. When the strip is pulled, the unsealed tail of the sample can hang down, flip up or be held. Each changes the peel angle at the seal, and each gives a different force. F88 therefore defines three techniques, requires you to pick one and use it consistently, and requires the technique to be reported with the results.

Technique A: unsupported

Each tail is clamped in an opposing grip and the seal is left to find its own position. The strip forms a T as it opens, and the peel angle changes as the stiffer side bends. Technique A is the most widely used in medical pouch testing, needs no fixture or hand, and is easy to automate. Its weakness is that the free seal can rotate or flip, especially with materials of very different stiffness, so operator setup and centring matter. Record any tail movement or flipping with the results.

Technique B: supported at 90° by hand

Each tail is clamped in an opposing grip, and the operator lightly supports the seal at 90° to the tails during the test, with loose contact that only stops the seal from swinging. This holds a near-constant 90° peel geometry. It is simple, but the result depends on the operator's hand, which makes Technique B harder to transfer between labs and shifts.

Technique C: supported at 180°

The less flexible tail is held flat against a rigid alignment plate clamped in one grip, and the more flexible tail is folded back 180° over the seal and clamped in the opposing grip. This is the configuration for lidding on rigid or semi-rigid trays and for any combination where one side is much stiffer than the other. It gives the most stable peel angle and usually the most repeatable result, but it measures a 180° peel, which reads differently from a T-peel of the same seal.

Which technique should you use?

  • Use the technique in your specification or validation protocol if it names one.

  • Technique A for routine pouch and bag testing where both sides are flexible and of similar stiffness, and when you want to avoid operator influence.

  • Technique B when the free seal flips badly under Technique A; train operators to keep the contact light.

  • Technique C for lidding peeled from trays and flanges, for stiff laminates, and when one side is much less flexible than the other.

  • Never compare results from different techniques or change technique mid-study.

The videos above show the T-peel and 180° peel geometries behind Techniques A and C on adhesive specimens; the centring and grip choices carry straight over to seal strips. See also our peel test fixtures guide.

ASTM F88 specimens: width, length and cutting

F88 allows three strip widths: 25 mm, 15 mm and 25.4 mm (1.00 in). Results are normalized by width, but you still cannot mix widths freely, because the edges of a cut strip behave differently from the middle and the normalization is not perfect. Pick one width for a product and stay with it.

  • 25 mm or 1 in is the usual choice in North America and for most medical pouch and tray validations.

  • 15 mm matches EN 868-5 and many European specifications, so it is used when one set of strips must satisfy both standards.

  • Length: tails long enough to clamp securely on both sides of the seal. A common layout is roughly 75 mm plus the seal width, but small pouches and narrow tray flanges often limit it.

  • Direction: cut the strip perpendicular to the seal so the seal line runs straight across the strip. A seal that crosses the strip at an angle peels at an angle and reads high.

  • Location: take strips from each seal of the package (for a pouch, typically each side, the chevron and the factory and customer seals) and keep each location as a separate data set. Corners, chevrons and overlap zones behave differently from straight seals.

Cutting strips cleanly

A strip with a ragged or nicked edge starts a tear at the edge instead of a peel at the seal, and that shows up as a material break or a low, scattered result. The cut edge must be clean and parallel.

  • Use a precision strip cutter or a sharp cutting die rather than scissors. A twin-blade strip cutter set to 25 mm or 15 mm gives parallel edges in one stroke.

  • Cutting dies: for high-volume work, a strip die cut on an arbor press or sample die press gives identical strips every time. See our cutting dies page and ask us about a strip die sized to your package.

  • Do not stretch the strip while cutting, and do not touch or crease the seal area.

  • Check width: a 24 mm strip calculated as 25 mm understates seal strength by 4 %.

Conditioning and sample history

  • Standard atmosphere: where conditioning is required, F88 refers to ASTM E171, the practice for conditioning and testing flexible barrier packaging (23 °C and 50 % relative humidity is the usual standard laboratory atmosphere). Paper and Tyvek lidding and paper-based laminates are humidity-sensitive, so condition them.

  • Time after sealing: seals can change for hours as the sealant crystallizes, so use a fixed, recorded delay before testing.

  • Sterilization and aging: for medical packaging, test before and after each sterilization cycle (EtO, gamma, e-beam, steam) and after accelerated aging (ASTM F1980) or real-time aging at each shelf-life time point. Aging is done on whole packages in an oven or climatic cabinet; the strips are cut afterwards.

  • Handling: cut strips from packages just before testing, keep them flat and away from heat sources, and handle by the tails only.

ASTM F88 test speed and machine requirements

F88 calls for a constant rate of grip separation of 200 to 300 mm/min (8 to 12 in/min). Most labs standardize on 250 mm/min (10 in/min) or 300 mm/min (12 in/min), and some align with EN 868-5's 200 mm/min so one method serves both standards. Whatever you choose, keep it constant across a validation, because many sealants and peelable coatings open at a higher force at a higher rate.

  • Force range: seal strengths of 1 to 10 lbf/in on a 25 mm strip correspond to roughly 4 to 45 N. Weak peelable seals can be under 5 N, while fusion seals on heavy laminates can approach the tensile strength of the film. Size the load cell for the strongest seal you test, then make sure the weakest seal still sits well within the cell's verified range.

  • Resolution: at a few newtons, the noise floor, the tare and drag from cables or hoses matter. A low-capacity load cell (for example 50 to 500 N) gives far better results than a 5 kN cell on the same frame.

  • Data rate: peelable seals open in small stick-slip events; 100 Hz or more captures the true peak and plateau.

  • Software: peak and average force per unit width, plus a way to record failure mode and technique for each strip.

Which testing machine for ASTM F88: Mark-10 or Galdabini?

F88 forces are low and the test is simple, so most F88 testing in production and QC is done on a single-column tensile tester. The choice between a Mark-10 frame and a Galdabini universal testing machine comes down to volume, the range of other tests you run, and how much reporting and data handling you need.

Mark-10 tensile testers: the natural fit for F88 QC

A Mark-10 motorized test frame is an excellent match for F88. The forces are well within the smallest frame, the 200 to 300 mm/min speed sits inside the standard speed range, and the compact footprint suits a packaging line or a cleanroom-adjacent QC room.

  • 100 lb (F105): 100 lbF (about 450 N) capacity and 18 in (457 mm) of travel. The standard speed range runs to 13 in/min (330 mm/min), which covers the full F88 range of 8 to 12 in/min without the extended speed option. This is the model we recommend for most F88 labs, because it gives the best low-force resolution.

  • 300 lb (F305) and 500 lb (F505): the same 18 in travel and speed range, for labs that also run film tensile (ASTM D882), puncture (ASTM F1306) or heavier peel tests on the same frame.

  • 750 lb (F755) and 1,500 lb (F1505): 32 in (813 mm) of travel and 10 to 600 mm/min. More capacity than F88 needs; choose them only if the same frame will run heavier work.

  • All Mark-10 F-series frames hold speed to ±0.2 % of setting and sample load at 5,000 Hz, so stick-slip peaks on peelable seals are captured cleanly.

Mark-10 F505-EM 500 lb tensile tester used for ASTM F88 seal strength testing of pouch strips

With a low-capacity force sensor and rubber-faced grips, a Mark-10 F105 is a complete F88 station for incoming inspection, sealer qualification and lot release. Compare the two machine types in Mark-10 test frame vs. universal testing machine.

Galdabini universal testing machines: advanced packaging labs

A Galdabini benchtop universal testing machine is the better fit when one frame must cover F88 alongside a broad packaging and materials program, when the lab needs full method libraries with automatic reports, or when seals must be tested at controlled temperature.

  • 2.5 kN Quasar: a single-column frame with up to 1,000 mm/min and 1 m of stroke. The open front makes strip loading fast, and the stroke also covers highly extensible films under ASTM D882.

  • 5 kN Quasar: a dual-column frame with 175 mm of column clearance, for labs that want room for an environmental chamber and wider fixtures.

  • 10 kN Quasar: for labs that combine packaging with plastics, adhesives and heavier components on one frame; pair it with a low-capacity load cell for the seal work.

With UTM software you can store separate F88 methods for each package, seal location and technique, define the averaging window once so every operator uses the same one, record the failure mode from a pick list, and export results for statistical process control. Read the universal testing machine buyer's guide for sizing.

A hand-cranked manual tensile tester is handy for go/no-go checks on the line, but it cannot hold a constant 200 to 300 mm/min, so it is not a compliant F88 setup. Use a motorized frame for validation and release data.

Grips for ASTM F88: pneumatic, vise and roller grips

Seal strips are thin, slippery and easy to tear at the jaw. The grip has to hold the tail without slipping or cutting it, close square so the seal line stays perpendicular to the pull, and not drag on the load cell. Rubber-coated or rubber-faced jaws are recommended so the jaw does not start a tear in the film.

Pneumatic grips

Pneumatic grips are the first choice for F88 in most labs. Air pressure sets the same clamping force on every strip, the jaws close square, and a foot pedal leaves both hands free to centre the seal. Our 2.4 kN centric and 2.6 kN pneumatic grips for elastomers and films have ample capacity and use a foot pedal. Set the air pressure only as high as needed to stop slipping, and clip the hose to the crosshead so it does not add drag to the reading.

Vise grips

Screw-action vise grips with rubber faces are a good, low-cost choice when volume is modest, because seal forces are low. Clamping force depends on the operator, so tighten consistently; strips that tear at the jaw edge mean the faces are too hard or the jaw is over-tightened. A vise is also the simplest way to hold an alignment plate for Technique C.

Roller grips

Self-tightening roller grips need no air supply and grip harder as the pull rises, which suits Tyvek, paper and heavier laminate tails on a Mark-10 frame. On very thin films, the line contact of the roller can pinch or nick the tail, so test a few strips first and switch to flat rubber-faced pneumatic or vise jaws if strips break at the grip.

Jaw faces, alignment and the Technique C plate

  • Jaw width: at least as wide as the strip, so the full width is clamped evenly. 25 mm to 50 mm faces suit 15 mm and 25 mm strips.

  • Faces: smooth rubber or rubber-coated faces for films and coated papers; avoid serrated faces, which bite and start tears.

  • Centring: the seal must sit midway between the jaws with the seal line perpendicular to the direction of pull. A centring device or a marked jaw speeds this up and reduces operator effect.

  • Slack: leave a small amount of slack so the seal is not loaded before the test starts, then zero the load cell.

  • Technique C: hold the less flexible tail flat against a rigid alignment plate in one grip and fold the flexible tail 180° into the other. The plate must stay parallel to the line of pull. Contact us about an alignment plate to suit your grips.

  • Adapters: our grips fit Instron, MTS, ZwickRoell, Shimadzu, Tinius Olsen and Mark-10 frames with the right grip adapters. See every option on the tensile grips page and the peel fixtures page.

Do you need an extensometer for ASTM F88?

No. F88 seal strength is a force divided by strip width. The standard does not measure strain or elongation, and crosshead position is all you need to plot force against grip separation and to define the averaging window. Nothing in the test is improved by clipping a contact extensometer to a seal strip, and you should not buy one for F88.

Where strain measurement does earn its place is on the rest of the flexible-packaging test program that usually shares the same frame:

  • Film tensile testing (ASTM D882): modulus and elongation of thin film should be measured on the specimen, not from the crosshead, and a non-contact video extensometer does this without loading or nicking the film. The UGC-VE-2109 gives a 220 mm field of view at ISO 9513 Class 0.5 and 440 mm at Class 1, enough for most film specimens to break.

  • Documenting failure modes: the camera of a video system can record every strip, which is useful evidence when a failure mode is disputed or a validation is audited.

  • Testing inside a chamber: a video extensometer looks through the chamber window, so film tensile tests at temperature need no contact hardware inside the chamber.

UGC-VE-2100 series single-camera video extensometer for ASTM D882 film tensile testing alongside F88 seal tests

For the full comparison of strain measurement options see types of extensometers and when should you use an extensometer.

ASTM F88 test procedure, step by step

  • Step 1: Define the technique (A, B or C), strip width, test speed, averaging window and seal locations in your protocol before you test anything.

  • Step 2: Condition the packages if required, then cut strips perpendicular to the seal at each location with a precision cutter. Label each strip with package, location and side.

  • Step 3: Inspect strips and discard any with nicked edges, wrinkles or visible channels in the seal; record the reason.

  • Step 4: Fit the low-capacity load cell, rubber-faced grips and, for Technique C, the alignment plate. Set the initial grip separation so the seal sits centred between the jaws, and clip any hoses and cables to the crosshead.

  • Step 5: Clamp the stiffer or package-side tail in the upper grip and the other tail in the lower grip (or as your protocol states), with the seal line perpendicular to the pull and a little slack in the strip. Zero the load.

  • Step 6: Run at the set speed (200 to 300 mm/min) until the seal has fully separated or the strip has broken. For Technique B, support the seal lightly at 90° throughout.

  • Step 7: Record the maximum force, the force trace and the failure mode for every strip, and note any tail movement or flipping.

  • Step 8: Calculate maximum seal strength and, if required, average seal strength per unit width, and summarize each seal location separately.

Reading the force trace and failure modes

The F88 result is incomplete without the failure mode. Two strips with the same peak force can mean very different things: one a clean peel at the design force, the other a weak seal that only reached that force because the film stretched before it tore. Classify every strip. Common categories are:

  • Adhesive (peel) failure: the two layers separate cleanly at the seal interface. This is the intended mode for peelable medical and food seals.

  • Cohesive failure: the sealant layer itself splits, leaving sealant on both faces. Common with some peelable coatings and intended in some designs.

  • Delamination: a laminate separates between its own layers inside or next to the seal, so you measure the laminate bond, not the seal.

  • Material tear or break at the seal edge: the web breaks at the edge of the seal before the seal opens, typical of fusion (lock-up) seals and over-sealed peelable seals. The peak force then reflects the material, not the seal.

  • Material break away from the seal or at the grip: usually a cutting or gripping problem; the strip is invalid for seal strength.

  • Elongation: the material stretches significantly before the seal opens or breaks, so the force trace shows a long ramp.

  • Fiber tear on Tyvek or paper: fibres pulled from the porous web, a sign of an over-sealed or too-aggressive seal and a particulate risk in sterile packaging.

Peelable seals usually rise to a first peak and then run along a plateau with small stick-slip peaks, which is what average seal strength describes. Fusion seals show a single rise to a break. A sudden drop to near zero partway through the peel points to a channel or skip and should be investigated, not averaged.

ASTM F88 calculations and worked example

  • Maximum seal strength: S(max) = F(max) ÷ w, where F(max) is the highest force recorded during separation and w is the strip width. This is the primary F88 result.

  • Average seal strength: S(avg) = F(avg) ÷ w, where F(avg) is the mean force over a defined portion of the peel. F88 does not fix a single averaging window, so state the one you use. Many labs exclude the first and last part of the separation (for example averaging between 10 % and 90 % of the peel) to remove the start-up and end effects.

  • Energy to separate (optional): the area under the force-displacement curve, sometimes reported per unit width for peel-only failures.

  • Units: report N/25 mm, N/15 mm or lbf/in, matching the strip width. 1 lbf/in = 4.378 N/25 mm = 2.627 N/15 mm. Never mix units from different strip widths without converting.

Worked example (25 mm strips, Technique A, 250 mm/min): strip 1 from the side seal of a film/Tyvek pouch peels cleanly and reaches a maximum force of 18.6 N. Maximum seal strength = 18.6 N per 25 mm, or 18.6 ÷ 4.378 = 4.25 lbf/in. The average force between 10 % and 90 % of the peel is 14.2 N, so average seal strength = 14.2 N/25 mm, or 3.24 lbf/in.

Five strips from the same seal give maximum seal strengths of 4.25, 4.10, 4.42, 3.96 and 4.31 lbf/in. The mean is 21.04 ÷ 5 = 4.21 lbf/in and the standard deviation is 0.18 lbf/in (a coefficient of variation of about 4 %). All five failed by adhesive peel. Against a minimum of 1.0 lbf/in and a maximum of 6.0 lbf/in, the seal passes with a wide margin on both sides.

Converting a European limit: EN 868-5 sets a minimum of 1.5 N per 15 mm for pouches intended for steam sterilization. On a 25 mm strip that is 1.5 × 25 ÷ 15 = 2.5 N/25 mm, or 0.57 lbf/in. The 1.2 N/15 mm minimum for other sterilization processes is 2.0 N/25 mm, or 0.46 lbf/in.

Typical seal strength values

  • Peelable medical pouches and header bags (film to Tyvek or paper): commonly about 1 to 5 lbf/in (roughly 4 to 22 N/25 mm). Many companies set a lower limit around 1 lbf/in and an upper limit chosen so the pouch opens without tearing or fibre tear.

  • Peelable lidding on trays and cups: similar to pouches, set by the peel force consumers or clinicians can manage.

  • Fusion (lock-up) seals on non-peelable packages: often limited by the strength of the film itself, so the strip breaks at the seal edge rather than peeling.

  • Treat these as orientation only. The seal design, sealant, technique and averaging method all move the numbers, and only your own validated limits count.

Sample size, precision and scatter

F88 does not prescribe a fixed number of strips. The number comes from your sampling plan and from the confidence you need in the result. Process validation programs typically test many strips per seal location at each condition (before and after sterilization, and at each aging time point), and statistically based plans such as attribute or variables sampling set the count for routine release. As a minimum for any comparison, test at least five strips per location and report the mean, standard deviation and range.

Between-lab differences in F88 are dominated by the technique, tail handling, strip cutting, grip pressure and the averaging window, not by the frame. A 10 % difference between two seals tested in one lab with one technique may be real; the same difference between two labs that have not agreed on technique, width, speed and averaging is not evidence of anything. Agree all of them in writing before you compare data with a supplier or contract lab. ASTM F3263 gives guidance on validating packaging test methods.

Testing seal strength at temperature

F88 is run at ambient laboratory conditions, and most specifications only require that. Two situations call for more:

  • Aging and sterilization are done on whole packages in ovens, climatic cabinets or sterilizers; the strips are tested at room temperature afterwards, so no chamber on the tester is needed.

  • Seal strength at service temperature: cold-chain, frozen-food, retort and hot-fill packaging is sometimes tested at the temperature it sees in use, by agreement between supplier and customer. Fit an environmental chamber to the frame (ours run from −80 to +280 °C), soak strips at temperature and test them inside the chamber.

  • Hot tack is a different test. The strength of a seal while it is still hot from the sealer is measured with a dedicated hot-tack method (ASTM F1921), not with F88.

What to report

  • The standard and edition (ASTM F88/F88M-xx) and the technique used (A, B or C).

  • Package and material description, seal location and side, and the sealing conditions if known.

  • Strip width, the cutting method and the number of strips tested and discarded, with reasons.

  • Conditioning, sterilization and aging history, and the test temperature.

  • Test speed, grip separation and grips used.

  • Maximum seal strength for each strip, with mean, standard deviation and range per seal location.

  • Average seal strength if required, with the averaging window or algorithm.

  • The failure mode of every strip, and any tail movement or flipping during the test.

Common ASTM F88 problems and how to fix them

  • Mixing techniques: one operator holds the tail, another lets it hang. Write the technique into the method and the software, and train to it.

  • Strips that break at the grip: hard or serrated faces, too much air pressure or a nicked edge. Use rubber faces, reduce pressure and improve cutting.

  • Seal not centred, not square or preloaded: use a centring device or marked jaws and leave a little slack.

  • Hose and cable drag: clip them to the crosshead.

  • Oversized load cell: a 5 kN cell reading 5 N is working at 0.1 % of capacity. Use a 50 to 500 N cell for seal work.

  • Undefined averaging: fix the window in the method and report it.

  • Ignoring failure mode: a strip that tore at 4 lbf/in is not the same as a seal that peeled at 4 lbf/in. Record the mode for every strip.

  • Speed outside the range: confirm the frame holds 200 to 300 mm/min under load.

ASTM F88 vs. EN 868-5, ISO 11607 and related ASTM methods

  • EN 868-5 (seal strength annex): the European method for heat-sealable pouches and reels uses 15 mm strips at 200 mm/min and sets minimum seal strengths of 1.5 N/15 mm (steam sterilization) and 1.2 N/15 mm (other processes). Running F88 at 200 mm/min on 15 mm strips lets one test serve both, but report against each standard separately.

  • ISO 11607-1 and -2: the international standards for packaging of terminally sterilized medical devices. They require seal strength to be specified and validated but do not define the test; F88 is the method most commonly referenced.

  • ASTM F2824: mechanical seal strength of round cups and bowl containers with flexible peelable lids, where the whole lid is peeled from the container instead of cutting strips.

  • ASTM F1140 and F2054: burst and creep testing of whole packages by internal pressure. They test every seal at once and complement F88.

  • ASTM F1929 and F2096: dye penetration and bubble leak tests for seal integrity, which find channels F88 can miss.

  • ASTM F2029: making laboratory heat seals to build a seal curve, often paired with F88.

  • Peel tests for adhesives and tapes: ASTM D903, ASTM D1876 and ASTM D3330 use the same 180° and T-peel geometries on bonded joints and tapes.

The film tests that usually share an F88 frame are ASTM D882 tensile, ASTM F1306 puncture, ASTM D1938 trouser tear and ASTM D1894 coefficient of friction. See our peel testing and puncture testing pages and the plastic film testing guide.

Complete ASTM F88 equipment packages

Basic QC station

  • Mark-10 F105 (100 lbF) tensile tester; 200 to 300 mm/min is within its standard speed range

  • Rubber-faced pneumatic grips with foot pedal, or rubber-faced vise grips for lower volumes

  • A precision 25 mm or 15 mm strip cutter, or a strip die on an arbor press

  • An alignment plate if you test lidding by Technique C

Advanced packaging lab

ASTM F88 FAQ

What is ASTM F88?

The ASTM test method for seal strength of flexible barrier materials. A strip cut across a seal is pulled apart at a constant rate, and the maximum force per unit width and the failure mode are reported.

What are Techniques A, B and C in ASTM F88?

How the tail is held: A unsupported, B supported by hand at 90°, C with the less flexible tail flat on an alignment plate and the other folded 180°. They give different values, so use one consistently and report it.

What specimen width does ASTM F88 use?

25 mm, 15 mm or 25.4 mm (1.00 in), cut perpendicular to the seal. 25 mm or 1 in is most common in the US; 15 mm matches EN 868-5.

What is the ASTM F88 test speed?

A constant rate of grip separation of 200 to 300 mm/min (8 to 12 in/min). Many labs use 250 or 300 mm/min, and some use 200 mm/min to align with EN 868-5.

How is seal strength calculated?

Maximum seal strength is the maximum force divided by the strip width, for example 18.6 N on a 25 mm strip is 18.6 N/25 mm or 4.25 lbf/in. Average seal strength uses the mean force over a defined part of the peel, and the averaging method must be stated.

What is a good seal strength for a medical pouch?

There is no single number in F88; limits come from your validation. Peelable medical pouches commonly fall between about 1 and 5 lbf/in, and EN 868-5 sets minimums of 1.5 N/15 mm for steam sterilization and 1.2 N/15 mm for other processes.

How many specimens should I test?

F88 does not set a fixed number. Your sampling plan and validation protocol decide it. Test strips from every seal location, at least five per location for any comparison, and many more for process validation.

What failure modes does ASTM F88 record?

Adhesive peel at the interface, cohesive failure in the sealant, delamination, material tear or break at the seal edge, elongation, and fibre tear on Tyvek or paper. Record the mode for every strip.

Can I run ASTM F88 on a Mark-10 tester?

Yes. The Mark-10 F105 is an ideal F88 frame: 100 lbF capacity for good low-force resolution, and its standard speed range to 330 mm/min covers 200 to 300 mm/min without the extended speed option.

What grips are best for ASTM F88?

Rubber-faced pneumatic grips with a foot pedal are the first choice. Rubber-faced vise grips work well at lower volumes, and roller grips suit Tyvek, paper and heavier laminates. Avoid serrated faces, which start tears.

Do I need an extensometer for ASTM F88?

No. Seal strength is force divided by width. An extensometer only earns its place if the same frame runs film tensile tests such as ASTM D882.

What is the difference between ASTM F88 and ASTM F2824?

F88 tests strips cut across a seal. F2824 peels the whole flexible lid from a round cup or bowl container, so it tests the complete seal as the consumer opens it.

Related reading

Get a complete ASTM F88 system

Universal Grip supplies everything for ASTM F88 seal strength testing: Mark-10 tensile testers sized for low seal forces, Galdabini universal testing machines for full packaging labs, rubber-faced pneumatic, vise and roller grips, peel fixtures, cutting dies and arbor presses for strip cutting, environmental chambers and video extensometers for the film side of the lab. Contact us with your package, seal locations, technique and strip width, and we will configure a system and quote it.