ASTM D2344 Complete Guide: Short-Beam Shear Specimens, 4:1 Span, Fixtures and Failure Modes
Updated: Nov 10
ASTM D2344 is the short-beam shear test for polymer matrix composites, the quickest way to check interlaminar strength, cure and porosity on a laminate. A small, thick coupon is bent over a span only four times its thickness until the plies slide apart. It needs a tiny specimen, a simple fixture and a few minutes per test, which is why it appears in almost every prepreg specification, incoming-material plan and process-control program. It is also easy to get wrong: a span set 1 mm off, an off-centre specimen, a worn loading nose or a failure mode read wrongly turns a valid interlaminar shear value into a number that means nothing. This complete guide covers specimen geometry and the 4:1 span rule, the 6 mm loading nose and 3 mm supports, specimen preparation and conditioning, the 1.0 mm/min test speed, which testing machine to use (a Mark-10 tester or a Galdabini universal testing machine), fixtures, why you do not need an extensometer and where video or DIC still helps, the calculation with a worked example, failure-mode classification, hot/wet testing, ISO 14130 and the other composite shear methods, troubleshooting and a full FAQ, with videos from our lab.
For the standard reference page and fixture details, see our ASTM D2344 short beam shear page. For how D2344 compares with the V-notch and ±45° methods, read composite shear testing: ASTM D2344 vs. D5379 vs. D7078 and D3518. This article focuses on running the test and choosing the equipment.
ASTM D2344 at a glance
Full title: Standard Test Method for Short-Beam Strength of Polymer Matrix Composite Materials and Their Laminates. The current edition is D2344/D2344M-22.
What it measures: short-beam strength, Fsbs, often called apparent interlaminar shear strength (ILSS), in MPa (psi).
Materials: continuous- or discontinuous-fiber polymer matrix composites whose elastic properties are balanced and symmetric about the beam axis, in flat or curved form.
Specimen: thickness h from 2.0 to 6.0 mm (0.08 to 0.25 in); width b = 2.0 × h; length = 6.0 × h. A 4 mm laminate gives a 24 × 8 × 4 mm coupon.
Span: 4.0 × thickness, the defining ratio of the method.
Loading nose and supports: 6.00 mm and 3.00 mm diameter cylinders in D2344M (0.250 in and 0.125 in in D2344), hardened to 60 to 62 HRC.
Speed: 1.0 mm/min (D2344M) or 0.05 in/min (D2344).
Stop the test at a 30 % load drop from maximum, a two-piece failure, or head travel greater than the nominal specimen thickness.
Result: Fsbs = 0.75 × Pm ÷ (b × h). At least five specimens per condition, each with its failure mode.
Typical equipment: a short-beam shear fixture on a 5 to 25 kN testing machine, with a load cell that resolves 0.5 to 12 kN well.

What ASTM D2344 measures and who uses it
In a laminate, the plies are held together only by the matrix. Interlaminar shear strength is how much shear stress that resin-rich layer can carry before the plies slide past each other. It is controlled by the resin, the fiber-matrix bond, the cure and, above all, porosity. A laminate with good fibers but voids, poor consolidation, contamination between plies or an incomplete cure shows it first in short-beam strength.
D2344 drives that failure with a three-point bend over a very short span. In a beam, bending stress grows with span while shear stress does not, so shortening the span to four times the thickness makes interlaminar shear fail before the outer plies break in bending. Typical users:
Prepreg and resin suppliers use it for batch acceptance and data sheets.
Aerospace, wind energy, automotive, marine and sporting-goods manufacturers use it to qualify materials, check cure cycles and monitor autoclave, oven and out-of-autoclave processes.
Repair and process engineers use it to compare cure schedules, layups and surface treatments, and to check panels after hot/wet ageing.
Universities and research labs use it to screen new resins, fiber sizings and nanoparticle-toughened systems on small panels.
The standard is clear about its limits. The stress state is not pure shear, especially under the loading nose, and failures are influenced by resin and interlaminar properties together. Short-beam strength is excellent for quality control, process specifications and comparison when specimens fail consistently in the same mode, but it is not a design shear allowable. For design shear properties use ASTM D5379, ASTM D7078 or ASTM D3518.
ASTM D2344 specimen dimensions
D2344 does not use one fixed coupon. Every dimension is a multiple of thickness, so the geometry stays the same for any laminate from 2 to 6 mm thick:
Thickness (h): 2.0 to 6.0 mm (0.08 to 0.25 in). Below 2 mm the specimen is too small to make and measure accurately.
Width (b): 2.0 × h.
Length: 6.0 × h, which leaves an overhang of one thickness beyond each support.
Span: 4.0 × h.
Worked sizes for common laminate thicknesses:
2 mm laminate: 12 × 4 × 2 mm, 8 mm span.
3 mm laminate: 18 × 6 × 3 mm, 12 mm span.
4 mm laminate: 24 × 8 × 4 mm, 16 mm span.
6 mm laminate: 36 × 12 × 6 mm, 24 mm span.
The fiber direction matters. For unidirectional tape, the 0° fibers run along the specimen length. For laminates, the layup must be balanced and symmetric about the beam axis, and you should report the stacking sequence, because short-beam strength depends on it. Curved specimens cut from tubes, spars or radii are covered too, with a support arrangement that depends on the ratio of radius to thickness; they need a fixture built for the curvature.
Why the 4:1 span is non-negotiable
The maximum shear stress in a three-point beam is 0.75 P ÷ (b h), while the maximum bending stress is 3 P S ÷ (2 b h²). With S = 4h, the bending stress is exactly eight times the shear stress. At 100 MPa of short-beam strength, the outer plies are carrying about 800 MPa in bending. That is comfortably below the flexural strength of unidirectional carbon/epoxy, so the plies shear first. Increase the span to 5h and the bending stress rises to ten times the shear stress, so weaker or woven laminates may break in flexure instead, and the result is no longer a shear value. This is why a span set to a round number rather than 4.0 × h is the most common D2344 error.
Specimen preparation
Machining: cut with a water-cooled diamond saw or abrasive wheel, following ASTM D5687 guidance where practical. Avoid heat, delamination at the cut edges and frayed fibers.
Edges: smooth, square and parallel. Edge damage starts delaminations at the overhang and lowers results.
Location: cut specimens from the panel area you want to evaluate, away from panel edges and bleeder marks, and record where each came from. Short-beam scatter often maps porosity across a panel.
Surfaces: leave tool and bag surfaces as made, but remove loose resin flash that would rock the specimen on the supports.
Measurement: measure width and thickness near the centre of the specimen, where the nose loads it, to about 0.025 mm (0.001 in). Use a micrometer with a 4 to 7 mm ball anvil on textured bag surfaces and a flat anvil on smooth ones.
Identification: mark specimens on the overhang, not in the span, and keep the tool-side face consistent if your specification requires it.
Porosity has a large effect on interlaminar shear, which is exactly why D2344 is used to detect it. If a batch reads low, check void content (ASTM D2734 or D3171) and cut a section for microscopy before blaming the resin.
Conditioning
Condition specimens as your material specification requires, using ASTM D5229 for moisture conditioning. Many labs test "as fabricated" or after drying, plus a hot/wet condition after moisture equilibrium.
If no conditioning is specified, test at standard laboratory conditions of about 23 °C and 50 % RH and report what you used; check the tolerances in your edition and specification.
For hot/wet testing, keep specimens sealed after removal from the humidity chamber and test within a short, fixed time, because small specimens lose moisture quickly, especially once heated.
Report the conditioning procedure, moisture content if measured, and the test environment with every result.
ASTM D2344 test speed and machine requirements
The crosshead speed is 1.0 mm/min (D2344M) or 0.05 in/min, which is 1.27 mm/min (D2344). Most specimens fail within about a minute. With a stiff coupon a few hundredths of a millimetre of slack or seating is a large part of the trace, so the machine must hold a slow, steady speed from the first contact.
Force: short-beam loads rise with the square of thickness. Pm = Fsbs × b × h ÷ 0.75, and since b = 2h, Pm = 2.67 × Fsbs × h².
2 mm specimens: about 0.5 to 1.3 kN for strengths of 50 to 120 MPa.
3 mm specimens: about 1.2 to 2.9 kN.
4 mm specimens: about 2.1 to 5.1 kN.
6 mm specimens: about 4.8 to 11.5 kN.
Load cell: choose one where the expected peak sits well inside the verified range. Resolution at a few hundred newtons matters for 2 mm specimens.
Stiffness and alignment: the nose must come down square to the specimen and centred between the supports. A machine with good lateral stiffness and an aligned fixture keeps the nose from rocking.
Data rate: 10 Hz or more, to capture the load drop that marks interlaminar failure.
Which testing machine for ASTM D2344: Mark-10 or Galdabini?
Both machine families can run D2344. The choice depends on specimen thickness, how much other composite testing the frame must do, and whether you need temperature testing.
Mark-10 test frames: QC on thinner laminates
A Mark-10 motorized test frame with a short-beam fixture and the right adapter is a compact, economical QC station for thin laminates. Size it from the force list above:
500 lb (F505), about 2.2 kN: 2 mm specimens of any common composite, and 3 mm specimens up to about 90 MPa.
750 lb (F755), about 3.3 kN: 3 mm specimens of most materials.
1,500 lb (F1505), about 6.7 kN: specimens up to about 4 mm thick, including high-strength carbon/epoxy. 6 mm aerospace laminates can exceed it.
Speed: the standard speed range of every Mark-10 F-series frame starts well above 1.0 mm/min, so specify Mark-10's optional low-speed range when you order a frame for D2344.
All F-series frames hold speed to ±0.2 % and sample load at 5,000 Hz, so the load drop at failure is captured cleanly. The F105 and F305 are too small for most composite specimens. Compare the two machine types in Mark-10 test frame vs. universal testing machine.

Galdabini universal testing machines: composite labs
For qualification, hot/wet testing, research and labs that run D2344 alongside other composite methods, a Galdabini benchtop universal testing machine is the better fit:
5 kN: a dual-column frame with 175 mm of column clearance, for a dedicated short-beam and flexure station on laminates up to about 3 to 4 mm, with room for an environmental chamber.
10 kN: covers most D2344 work up to about 5 mm, plus ASTM D790 and D7264 flexure.
25 kN: the safe choice for 6 mm aerospace laminates at 120 MPa or more, with margin for thick flexure specimens.
50 kN and 100 kN: for labs that run D2344 on the same frame as ASTM D3039 tension, ASTM D6641 compression and D5379 or D7078 shear. Use a lower-capacity load cell for short-beam work to keep resolution.
UTM test software stores a D2344 method with the span, stop criteria and failure-mode field, calculates Fsbs from the measured width and thickness, and reports mean, standard deviation and coefficient of variation. See our universal testing machine buyer's guide and the composite test fixture buyer's guide.
Quick comparison
Choose a Mark-10 for production QC of laminates up to about 4 mm thick at room temperature, with the low-speed option and a small footprint.
Choose a Galdabini UTM for 6 mm laminates, hot/wet and cold testing from −80 to +280 °C, research and qualification, and one frame that also runs flexure, tension, compression and in-plane shear.
ASTM D2344 fixtures: loading nose, supports and span
D2344 needs no grips. The specimen sits on two support cylinders and a loading nose presses down at mid-span, so the fixture is a small, precise three-point bend jig mounted on the frame through adapters. What makes a good D2344 fixture:
Correct cylinders: a 6.00 mm loading nose and 3.00 mm supports for D2344M, or 0.250 in and 0.125 in for D2344, hardened to 60 to 62 HRC and finish ground. Worn, flattened or chipped cylinders change the contact stress and the failure mode.
Accurate span adjustment: a scale, gauge blocks or micrometer adjustment that sets 4.0 × h for every thickness you test, accurate to about 0.1 mm or better. On an 8 mm span, a 0.5 mm error is more than 6 %.
Centring: end stops or a rear fence that put the specimen centre under the nose and keep it square to the cylinders, with the overhang equal at both ends.
Alignment: the nose axis parallel to the supports and centred between them, with no rocking as load is applied.
Capacity: a fixture rated 10 to 20 kN covers almost all laminates.
Our ASTM D2344 short beam shear fixture comes with 6/3 mm or 0.250/0.125 in cylinders, micrometer span adjustment and a centring stop, with ISO 14130 and curved-beam options. See it with our other composite fixtures on the shear fixtures page and our three- and four-point fixtures on the bend testing fixtures page, including the small bend fixture with 4 to 150 mm spans and interchangeable rollers for D790 and D7264 flexure on the same frame.
What about grips?
Wedge, vise, pneumatic and roller grips are not used for D2344. Labs that run D3039 tension on the same frame use wedge or hydraulic grips for that test and swap to the bend fixture for short-beam work; a quick-change adapter system makes the swap fast.
Do you need an extensometer for ASTM D2344?
No. D2344 reports a strength calculated from the maximum load and the specimen dimensions. There is no modulus or strain in the result, so the standard does not require an extensometer. The load-displacement curve is recorded from the crosshead, which is enough to see the load drop and the shape of the failure. If you want a cleaner deflection trace, a deflectometer under the specimen measures mid-span deflection directly and removes machine and fixture compliance, but it is optional.
Where video and DIC do add value:
Reading the failure mode. The single most important judgement in D2344 is whether the specimen failed in interlaminar shear. A camera on the specimen edge records where the first crack started (at mid-thickness, near the nose or at the outer plies) and in what order things happened, which is far more reliable than inspecting a cracked coupon afterwards.
Strain mapping. A video extensometer used as a 2D DIC system on a speckled edge shows the shear strain concentrating at mid-thickness between nose and supports, and the compressive damage under the nose. This is valuable when comparing resins or explaining an inelastic failure.
Chamber testing. Through a heated chamber window, a video extensometer records hot/wet tests without opening the door.
The rest of the composite lab. The same camera measures D3039 modulus and Poisson's ratio, where strain measurement is required. A UGC-VE-2109 covers tensile coupons, and the 3D UGC-VE-4105 adds out-of-plane measurement.

Clip-on extensometers have no place on a 24 mm short-beam coupon. For when strain measurement is required and when it is not, read when should you use an extensometer and the video extensometer buying guide.
ASTM D2344 test procedure, step by step
Step 1: Cut at least five specimens per condition to 6h × 2h × h, with the fibers in the specified direction, and record their panel locations.
Step 2: Condition the specimens as specified and record the conditioning.
Step 3: Measure width and thickness near the centre of each specimen to about 0.025 mm.
Step 4: Set the support span to 4.0 × thickness and check it with a gauge. Check that the nose is centred and the cylinders are undamaged.
Step 5: Place the specimen on the supports against the centring stops, with equal overhang and the specified face up.
Step 6: Bring the nose into light contact, zero the load and displacement, and start the test at 1.0 mm/min (or 0.05 in/min).
Step 7: Record load against crosshead displacement. Stop at a 30 % load drop from the maximum, a two-piece failure, or head travel greater than the nominal thickness.
Step 8: Record the maximum load Pm, then examine the specimen edges, ideally under magnification, and classify the failure mode.
Step 9: Calculate Fsbs for each specimen and the mean, standard deviation and coefficient of variation for the set, noting any specimens with failures other than interlaminar shear.
ASTM D2344 calculation and worked example
Short-beam strength: Fsbs = 0.75 × Pm ÷ (b × h), where Pm is the maximum load observed during the test, b the measured width and h the measured thickness.
Units: N and mm give MPa; lbf and in give psi. Multiply MPa by 145.04 for psi.
Where 0.75 comes from: in a three-point beam, each half carries a shear force of P/2, and the parabolic shear distribution peaks at 1.5 times the average, so τmax = 1.5 × (P/2) ÷ (b h) = 0.75 P ÷ (b h), at mid-thickness.
Worked example: a nominal 4 mm carbon/epoxy laminate. The specimen measures b = 8.04 mm and h = 4.02 mm, so the span is set to 4.0 × 4.0 = 16 mm. The load rises almost linearly, then drops sharply at Pm = 4,310 N as a crack runs along the mid-plane. Fsbs = 0.75 × 4,310 ÷ (8.04 × 4.02) = 3,232.5 ÷ 32.32 = 100.0 MPa (about 14,500 psi).
Bending check: with S = 4h, the outer-ply bending stress is eight times the shear stress, about 800 MPa here, well below the flexural strength of this laminate, which is consistent with the interlaminar failure observed.
Set statistics: five specimens give 100.0, 97.6, 102.3, 99.1 and 96.8 MPa, all failing in interlaminar shear. The mean is 99.2 MPa, the standard deviation 2.2 MPa and the coefficient of variation 2.2 %.
Typical short-beam strength values
Approximate ranges from published data for well-made laminates, as a sanity check rather than a specification:
Unidirectional carbon/epoxy aerospace prepreg: roughly 90 to 130 MPa (13 to 19 ksi).
Woven carbon/epoxy: roughly 60 to 85 MPa.
Glass/epoxy: roughly 50 to 80 MPa.
Glass/polyester and glass/vinyl ester: roughly 25 to 50 MPa.
Carbon/thermoplastic (for example PEEK): roughly 80 to 110 MPa, though tough matrices often deform inelastically instead of shearing cleanly.
A drop of 10 % or more from a material's usual value is worth investigating: porosity, under-cure, moisture, contamination between plies or the wrong span are the usual causes.
Failure modes: what makes a valid short-beam result
D2344 requires the failure mode of every specimen to be identified and reported, and the standard illustrates the typical modes. They fall into three families:
Interlaminar shear (valid): one or more cracks run along ply interfaces between the nose and a support, usually near mid-thickness. Single-crack and multiple-crack shear failures both count, and the load trace shows a clear, sharp drop.
Flexure: fibers break on the tension face under the nose, or plies buckle or crush on the compression face. The specimen failed in bending, so the value is not an interlaminar shear strength.
Inelastic deformation: the matrix yields, the nose indents, and the curve rounds over with no clear drop. Common with thermoplastic and highly toughened matrices. Pm is then a deformation limit, not a shear strength.
Combinations: for example a compression failure under the nose followed by interlaminar cracks. Classify by what happened first, which is where video helps.
Report the strength and mode for every specimen. Most specifications use only interlaminar shear failures as valid short-beam strength values and report the others separately, rather than mixing them into the average. If most specimens fail in flexure or inelastic deformation, D2344 is the wrong test for that material, or the span is wrong; check the span and consider ISO 14130, D5379 or D7078 instead.
Precision and scatter
Short-beam results are repeatable for a given material, geometry and stacking sequence when specimens fail consistently in the same mode, which is why D2344 works so well for QC. Well-made aerospace laminates commonly give coefficients of variation of only a few percent. A CV above about 10 % usually points to the specimens, not the material: porosity varying across the panel, inconsistent thickness, edge damage, or a mix of failure modes. Fixture problems such as a wrong span, a worn nose or off-centre specimens also show up as scatter. Check the current edition for any interlaboratory precision data.
Testing short-beam strength at temperature and hot/wet
Matrix-dominated properties fall at elevated temperature, especially after moisture conditioning, so aerospace qualification usually runs D2344 at room temperature, cold, hot and hot/wet conditions.
Use an environmental chamber on the frame; ours run from −80 to +280 °C. Place a thermocouple on or beside a dummy specimen and soak for the time your specification requires.
Use a fixture rated for the temperature. High-temperature bend fixtures in heat-resistant alloy with long extension rods keep the frame and load cell outside the hot zone.
For hot/wet tests, minimise the time from humidity chamber to test, because small specimens dry out quickly at temperature, and report the moisture content if measured.
See the temperature chamber buyer's guide and aerospace composite testing for hot/wet setups.
What to report
The standard and edition, D2344 or D2344M, and any deviations.
Material, fiber and matrix, stacking sequence, panel identification, fabrication and cure method, and void content if measured.
Specimen location in the panel, measured width and thickness, span and span-to-thickness ratio, and flat or curved geometry.
Loading nose and support diameters and the test speed.
Conditioning, moisture content if measured, test temperature and humidity.
Maximum load, short-beam strength and failure mode of each specimen.
Mean, standard deviation and coefficient of variation, stating which specimens were included.
Load-displacement curves where required.
Common ASTM D2344 problems and how to fix them
Wrong span: a fixed 10 mm or 20 mm span used for every thickness. Set 4.0 × h for each thickness group and check with a gauge.
Off-centre specimen: the nose lands nearer one support, raising shear on one side and changing the mode. Use centring stops and equal overhang.
Worn or wrong-diameter cylinders: a flattened nose crushes the top plies. Inspect regularly and replace damaged cylinders.
Flexure failures: too long a span, or a material with low flexural strength relative to its interlaminar strength. Check the span first.
Inelastic deformation: typical of tough thermoplastic matrices. Report it as such; the value is not ILSS.
Low, scattered values: porosity, poor consolidation or edge damage from cutting. Check void content and the saw.
Too fast: running at a default 5 or 10 mm/min. Use 1.0 mm/min.
Nominal dimensions in the formula: a laminate 3.85 mm thick instead of 4.00 mm changes the result by 4 %. Measure every specimen.
Overloaded frame: 6 mm carbon/epoxy can reach 12 kN. Size the machine and fixture from the thickest, strongest laminate you test.
Reporting Fsbs as a design shear strength: it is an apparent value for QC and comparison.
ASTM D2344 vs. ISO 14130 and EN 2563
ISO 14130 measures apparent interlaminar shear strength by the same short-beam principle and the same formula, but with a different geometry: a fixed 20 × 10 × 2 mm specimen, a 10 mm span (5:1), a 10 mm diameter loading nose and 4 mm diameter supports, at 1 mm/min. EN 2563 is the related European aerospace method, also on 2 mm laminates. The longer span ratio and larger cylinders change the stress state, so ISO and ASTM values are close but not interchangeable. Our D2344 fixture is available with an ISO 14130 option; report the standard with every result.
D2344: span 4h, 6 mm nose, 3 mm supports, thickness 2 to 6 mm, flat or curved.
ISO 14130: span 5h, 10 mm nose, 4 mm supports, 2 mm thick reference specimen, flat only.
ASTM D4475: the short-beam method for pultruded reinforced plastic rods.
Related composite tests
ASTM D5379: V-notched beam (Iosipescu) shear, giving in-plane or interlaminar shear strength and, with strain gauges, shear modulus.
ASTM D7078: V-notched rail shear, with a larger gauge area that suits textile composites.
ASTM D3518: ±45° tension for in-plane shear stress-strain response, run in tension grips on the ASTM D3039 setup.
ASTM D790 and D7264: flexural properties at long spans, the opposite end of the span-ratio scale. See 3-point vs. 4-point bend testing and ASTM D6272.
ASTM D6415: curved-beam interlaminar tensile strength, and ASTM D5528 and D7905: mode I and mode II delamination toughness.
ASTM C393 and ASTM C273: core shear of sandwich panels, which uses the same short-span principle on a sandwich beam. See sandwich panel testing.
For bonded joints rather than laminates, see the ASTM D1002 lap shear complete guide.
Complete ASTM D2344 equipment packages
Basic QC station
Mark-10 F1505 (6.7 kN) with the low-speed option, for laminates up to about 4 mm
ASTM D2344 short beam shear fixture with 6/3 mm cylinders, span adjustment and centring stop, plus adapters
A ball-anvil micrometer and a water-cooled diamond saw for specimen preparation
Advanced composite lab
Galdabini 25 kN UTM, or 50 kN to 100 kN to add D3039 and D6641 on one frame
D2344 fixture with ISO 14130 and curved-beam options, and bend fixtures for D790 and D7264
Shear fixtures for D5379 and D7078
Environmental chamber for −80 to +280 °C and hot/wet testing, with high-temperature fixture versions
UGC-VE-2109 video extensometer for D3039 strain, failure recording and DIC strain maps

ASTM D2344 FAQ
What is ASTM D2344?
The ASTM test method for short-beam strength of polymer matrix composites. A short coupon is loaded in three-point bending over a span of four times its thickness so it fails in interlaminar shear, and 0.75 × Pm ÷ (b × h) gives the short-beam strength.
What are the ASTM D2344 specimen dimensions?
Thickness 2 to 6 mm, width twice the thickness and length six times the thickness. A 4 mm laminate gives a 24 × 8 × 4 mm specimen tested on a 16 mm span.
What is the span-to-thickness ratio in ASTM D2344?
4.0. The span is four times the specimen thickness, which keeps bending stress at eight times the shear stress so the specimen fails in interlaminar shear rather than flexure.
What loading nose and support diameters does ASTM D2344 use?
A 6.00 mm loading nose and 3.00 mm supports in D2344M (0.250 in and 0.125 in in the inch-pound D2344), hardened to 60 to 62 HRC.
What is the ASTM D2344 test speed?
1.0 mm/min in D2344M, or 0.05 in/min (1.27 mm/min) in D2344. Stop at a 30 % load drop, a two-piece failure or head travel greater than the specimen thickness.
How is short-beam strength calculated?
Fsbs = 0.75 × Pm ÷ (b × h). For example, 4,310 N on an 8.04 × 4.02 mm specimen gives 0.75 × 4,310 ÷ 32.32 = 100.0 MPa.
Is short-beam strength the same as interlaminar shear strength?
It is often called apparent interlaminar shear strength, but the stress state is not pure shear, especially under the nose. It is a QC and comparison value, not a design shear allowable.
Which failure modes are valid in ASTM D2344?
Interlaminar shear, with one or several cracks along ply interfaces. Flexural tension or compression failures and inelastic deformation must be reported as such and do not give an interlaminar shear value.
How many specimens does ASTM D2344 require?
At least five per test condition, unless fewer give valid results, for example in a designed experiment. Report the failure mode of each.
Do I need an extensometer for ASTM D2344?
No. The result needs only maximum load and dimensions, and the curve comes from the crosshead or an optional deflectometer. Video or DIC helps identify the failure mode, map strain and record chamber tests.
What testing machine do I need for ASTM D2344?
Loads are about 0.5 to 1.3 kN on 2 mm specimens and up to about 12 kN on 6 mm carbon/epoxy. A Mark-10 F1505 with the low-speed option covers laminates up to about 4 mm; a 10 to 25 kN Galdabini UTM covers the full range.
What is the difference between ASTM D2344 and ISO 14130?
ISO 14130 uses a 20 × 10 × 2 mm specimen, a 5:1 span, a 10 mm nose and 4 mm supports; D2344 uses a 4:1 span, 6 mm nose and 3 mm supports on 2 to 6 mm laminates. The formula is the same, but results are not interchangeable.
Related reading
Composite shear testing: ASTM D2344 vs. D5379 vs. D7078 and D3518
Aerospace composite testing: shear fixtures, Galdabini UTMs and ASTM methods
3-point vs. 4-point bend testing: ASTM D790, D6272 and C1161
Types of extensometers: clip-on vs. video vs. long-travel vs. 3D DIC
More complete guides: ASTM D256 Izod impact, ASTM D903 180° peel, ASTM D1876 T-peel, ASTM F88 seal strength, ASTM D5035 strip tensile, ASTM D5034 grab tensile and ASTM D395 compression set
Get a complete ASTM D2344 system
Universal Grip supplies everything for ASTM D2344 and the rest of your composite program: short beam shear fixtures with ISO 14130 and curved-beam options, bend testing fixtures, V-notch and other shear fixtures, wedge and hydraulic grips for D3039 on the same frame, adapters, environmental chambers, video extensometers, and testing machines from a Mark-10 test frame to a full Galdabini universal testing machine. Tell us your laminate thicknesses, materials and temperature range, and we will configure a short-beam shear system and quote it. Contact us.




Comments